Lithium-rich manganese-based precursor for solid-state battery as well as preparation method and application of lithium-rich manganese-based precursor
Through gradient doping structure and coating layer technology, high-performance lithium-rich manganese-based cathode materials are prepared, which solves the problems of poor cycle performance and low rate performance of existing materials under high voltage, improves volume energy density and reduces Equipment costs.
Patent Information
- Application Number
- CN202410735342.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
AI Technical Summary
Existing lithium-rich manganese-based cathode materials have poor cycle performance under high voltage, low rate performance and low volumetric energy density. In addition, fluorine doping brings high equipment costs and easy material breakage.
Using a lithium-rich manganese-based precursor with a gradient doping structure, the Nb element gradient decreases from the inside to the outside, and the Co element gradient increases from the inside to the outside, forming a structure that is compact inside and loose outside. Coating technology prepares high-performance lithium-rich manganese-based cathode materials.
It improves the rate and cycle performance of lithium-rich manganese-based cathode materials, increases the volume energy density, reduces equipment costs, increases the contact area with the solid electrolyte, and improves the mechanical strength and compaction density of the material.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a lithium-rich manganese-based precursor for solid-state batteries, and a preparation method and application thereof. Background Art
[0002] Lithium-rich manganese-based positive electrode materials have high voltage characteristics and can provide higher energy density, which helps to improve the energy density of the battery, thereby increasing the driving range. The development of a 4.8V high-voltage electrolyte suitable for lithium-rich manganese-based positive electrode materials is a challenging task, which to a certain extent limits the performance of its high-voltage characteristics. Solid electrolytes can adapt to higher operating voltages. If paired with ternary positive electrode materials or lithium iron phosphate positive electrode materials, the room for improvement in energy density has become smaller and smaller. Therefore, lithium-rich manganese-based positive electrode materials are expected to become the best choice for future solid-state batteries.
[0003] In addition to the need for high voltage to achieve high capacity, lithium-rich manganese-based cathode materials also have several drawbacks: 1) During the cycle, Mn 3+ Migration into lithium vacancies causes the layered structure to transform into a spinel structure, resulting in a continuous decrease in the average discharge voltage, causing serious energy loss and posing huge challenges to battery management; 2) Poor rate performance; 3) Low material density, resulting in low volume energy density.
[0004] By regulating the morphology and structure of the lithium-rich manganese-based precursor, the performance of the lithium-rich manganese-based positive electrode material can be improved. For example, CN108557905A discloses a lithium-rich manganese-based material precursor and a preparation method thereof, a lithium-rich manganese-based positive electrode material and a preparation method thereof, and a lithium battery. The lithium-rich manganese-based material precursor is a lithium-rich manganese-based material carbonate precursor with a flake-like morphology. The particle size of the lithium-rich manganese-based material carbonate precursor with a flake-like morphology is 1 μm-7 μm, and the specific surface area is 8 m 2 / g-50m 2 / g. This method uses the lithium-rich manganese-based material precursor to prepare a single-crystal lithium-rich manganese-based positive electrode material with a higher degree of single crystallization with a simpler process and lower production cost, thereby improving the mechanical strength and compaction density of the microstructure of the positive electrode material, improving the capacity, initial efficiency and inhibiting voltage decay. However, compared with the hydroxide precursor, the positive electrode material obtained from the carbonate precursor is easy to produce gas, has low compaction, low strength and is easy to break. This invention reduces the impact of the carbonate precursor by burning single crystals, but the single crystal material has poor rate performance compared to the polycrystalline material, which has a negative impact on the lithium-rich manganese-based material with poor rate performance.
[0005] CN112234176A prepares a fluorine- and magnesium-co-doped lithium-manganese-based precursor by a dual-system coprecipitation method. The lithium-manganese-based positive electrode material prepared from the lithium-manganese-based precursor can effectively improve the material crystal stability and inhibit voltage decay, and the prepared lithium-ion battery has good electrochemical performance. However, in addition to the negative impact of carbonate precursors, the doping of fluorine is also a great challenge. Fluoride ions can corrode stainless steel equipment and are also easily volatilized at high temperatures. The production equipment material requirements for precursors and positive electrode materials are extremely high, which greatly increases the equipment investment cost.
[0006] Therefore, providing a lithium-rich manganese-based precursor so that the lithium-rich manganese-based positive electrode material prepared by using the precursor has good cycle performance, rate performance and high energy density is a technical problem that needs to be solved urgently. Summary of the invention
[0007] In view of the above problems existing in the prior art, the object of the present invention is to provide a lithium-rich manganese-based precursor for solid-state batteries and a preparation method and application thereof.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a lithium-rich manganese-based precursor for a solid-state battery, wherein the chemical formula of the lithium-rich manganese-based precursor is Ni x Mn y Nb a Co b (OH)2, wherein 0.25<x≤0.4, 0.6≤y<0.75, 0.001≤a<0.005, 0.005≤b<0.01, and x+y+a+b=1, the content of Nb element decreases gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside, and the structure of the lithium-rich manganese-based precursor is compact inside and loose outside.
[0010] In the lithium-rich manganese-based precursor of the present invention, the value range of x is 0.25<x≤0.4, and x can be, for example, 0.27, 0.3, 0.32, 0.35, 0.38 or 0.4; the value range of y is 0.6≤y<0.75, and y can be, for example, 0.6, 0.62, 0.64, 0.65, 0.68, 0.7, 0.72 or 0.73; the value range of a is 0.001≤a<0.005, and a can be, for example, 0.001, 0.002, 0.003 or 0.004; the value range of b is 0.005≤b<0.01, and b can be, for example, 0.005, 0.006, 0.007, 0.008 or 0.009.
[0011] The lithium-rich manganese-based precursor of the present invention has a specific gradient doping structure and a tight inner and loose outer structure. The lithium-rich manganese-based positive electrode material prepared by using the precursor can inherit the gradient doping structure and the tight inner and loose outer structural characteristics of the precursor. Among them, Nb doping can improve Li + The diffusion rate can be increased and the material structure can be stabilized, thereby improving the rate and cycle performance. Co doping can also stabilize the structure and improve the cycle performance. The compactness of the internal material can increase the density, thereby increasing the volume energy density, while the looseness of the external material can increase the contact area with the solid electrolyte and improve the rate performance.
[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0013] Preferably, the particle size D50 of the lithium-rich manganese-based precursor is 3 μm-3.5 μm, for example, 3 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm or 3.5 μm, etc. The lithium-rich manganese-based precursor has a smaller particle size, so the lithium-rich manganese-based positive electrode material formed therefrom also has a smaller particle size, which helps to improve the capacity and rate performance of the material.
[0014] As a preferred technical solution of the lithium-rich manganese-based precursor of the present invention, the outer surface of the lithium-rich manganese-based precursor is coated with a coating layer, and the coating layer includes cobalt hydroxide. Co enrichment on the outside can effectively reduce the residual alkali content.
[0015] Preferably, the coating layer has a thickness of 0.05 μm-0.1 μm, for example, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm or 0.1 μm.
[0016] In a second aspect, the present invention provides a method for preparing the lithium-rich manganese-based precursor as described in the first aspect, the preparation method comprising the following steps:
[0017] A coprecipitation reaction is carried out using a nickel-manganese salt solution, a Nb salt solution, a Co salt solution, a precipitant solution and a complexing agent solution. During the reaction, the content of the Nb element provided by the Nb salt solution and the Co salt solution is controlled to gradually decrease while the content of the Co element is gradually increased.
[0018] The method of the invention is simple and has good controllability. The element doping effect in the prepared lithium-rich manganese-based precursor is controllable, and the lithium-rich manganese-based positive electrode material prepared by the method has good performance.
[0019] Preferably, the coprecipitation reaction temperature is 40°C-80°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.
[0020] Preferably, the coprecipitation reaction is carried out under the protection of a protective gas.
[0021] Preferably, the protective gas includes at least one of nitrogen, helium and argon.
[0022] Preferably, the reaction is divided into an early reaction stage and a late reaction stage, wherein the early reaction stage is a stage from the generation of the precursor to the growth to a particle size D=(70%-85%)×D0, wherein D0 is a target particle size. For example, D may be 70%×D0, 72%×D0, 75%×D0, 77%×D0, 80%×D0, 82%×D0, or 84%×D0, etc.
[0023] Preferably, in the early stage of the reaction, the rotation speed of the coprecipitation reaction is 400 rpm-500 rpm, for example, it can be 400 rpm, 420 rpm, 440 rpm, 450 rpm, 460 rpm, 480 rpm or 500 rpm.
[0024] Preferably, in the early stage of the reaction, the pH value of the coprecipitation reaction is 11.0-12.0, for example, it can be 11.0, 11.2, 11.3, 11.4, 11.5, 11.6, 11.8 or 12.0.
[0025] Preferably, in the early stage of the reaction, the complexing agent is aqueous ammonia.
[0026] Preferably, in the early stage of the reaction, the ammonia concentration in the reaction system is 3.0 g / L-10.0 g / L, for example, it can be 3.0 g / L, 3.4 g / L, 4 g / L, 4.5 g / L, 5 g / L, 5.5 g / L, 6 g / L, 6.5 g / L, 7 g / L, 7.5 g / L, 8 g / L, 8.5 g / L, 9 g / L, 9.5 g / L or 10 g / L, etc.
[0027] Preferably, in the later stage of the reaction, the rotation speed of the coprecipitation reaction is 200 rpm-300 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm or 300 rpm.
[0028] Preferably, in the later stage of the reaction, the complexing agent is a sodium citrate solution.
[0029] Preferably, in the later stage of the reaction, the concentration of sodium citrate in the reaction system is 0.2 g / L-2 g / L, for example, it can be 0.2 g / L, 0.5 g / L, 1 g / L, 1.2 g / L, 1.4 g / L, 1.5 g / L, 1.7 g / L, 1.8 g / L or 2 g / L.
[0030] In the preparation method of the present invention, by adopting a high rotation speed and using ammonia water as a complexing agent in the early stage of the reaction, and adopting a low rotation speed and using a sodium citrate solution as a complexing agent in the later stage of the reaction, the structure of the lithium-rich manganese-based precursor can be adjusted, and the performance of the lithium-rich manganese-based positive electrode material prepared therefrom can be improved.
[0031] As a preferred technical solution of the method of the present invention, the method of controlling the Nb salt solution and the Co salt solution to gradually reduce the content of the Nb element and gradually increase the content of the Co element is:
[0032] A nickel-manganese salt solution, a Nb salt solution, a Co salt solution, a precipitant solution and a complexing agent solution are added to a reaction kettle in parallel, wherein the amount of the Nb salt solution is fixed, and the Co salt solution is added to the Nb salt solution at a certain rate.
[0033] Preferably, the certain rate is 0.1L / h-1L / h, for example, it can be 0.1L / h, 0.2L / h, 0.3L / h, 0.4L / h, 0.5L / h, 0.6L / h, 0.7L / h, 0.8L / h, 0.9L / h or 1L / h, etc.
[0034] Preferably, the pH value of the Nb salt solution and the Co salt solution is the same. The same pH value of the two can avoid pH fluctuations during the reaction due to different amounts of alkali consumed by the two.
[0035] Preferably, the method further comprises coating when the precursor grows to a particle size D0, wherein the coating method is: stopping the use of the Nb salt solution and retaining only the nickel manganese salt solution, the Co salt solution, the precipitant solution and the complexing agent solution for co-precipitation reaction.
[0036] Preferably, in the coating method, the pH value and the complexing agent concentration are stabilized by adjusting the strength of the precipitant solution and the complexing agent solution.
[0037] Preferably, in the coating method, the concentration of the Co salt solution is 1 g / L-10 g / L, for example, it can be 1 g / L, 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L or 10 g / L.
[0038] The present invention adopts a low-concentration Co salt solution and prolongs the coating time to carry out coating, thereby ensuring the coating uniformity of the Co element and forming a uniform coating layer on the particle surface.
[0039] Preferably, in the coating method, the coprecipitation reaction time is 10 h to 20 h, for example, it can be 10 h, 12 h, 13 h, 14 h, 15 h, 17 h, 18 h or 20 h.
[0040] Preferably, the method further comprises the steps of washing, drying, screening and iron removal of the product after coating.
[0041] As a preferred technical solution of the method for preparing the lithium-rich manganese-based precursor of the present invention, the method comprises the following steps:
[0042] Step 1, preparing a nickel-manganese mixed salt solution of a certain concentration according to a certain metal molar ratio; preparing a Nb salt solution and a Co salt solution of a certain concentration, and adjusting the pH values of the Nb salt solution and the Co salt solution with dilute sulfuric acid to make the pH values of the two the same;
[0043] Step 2, under a nitrogen atmosphere, adding a nickel-manganese salt solution, a Nb salt solution, a sodium hydroxide solution and an ammonia solution into a reaction kettle in parallel, wherein the amount of the Nb salt solution is fixed, and the Co salt solution is added to the Nb salt solution at a certain rate;
[0044] Step 3, the temperature of the reactor is controlled at 40°C-80°C throughout the reaction. In the early stage of the reaction, the speed of the reactor is controlled at 400rpm-500rpm, the pH is controlled at 11.0-12.0, and the ammonia concentration is controlled at 3.0g / L-10.0g / L. When the precursor particle size grows to 2.5μm, the speed of the reactor is reduced to 200rpm-300rpm, and the complexing agent is replaced with a sodium citrate solution. The concentration of sodium citrate is controlled at 0.2g / L-2g / L. When the precursor particle size grows to 3.0μm-3.5μm, only the Co salt solution, the sodium hydroxide solution and the sodium citrate solution are retained, and the feeding of other solutions is stopped, and the feeding flow rates of the sodium hydroxide solution and the citric acid solution are adjusted to keep the pH value and the concentration of the complexing agent stable. The feeding is stopped after the reaction for 10h-20h;
[0045] Step 4: Wash, dry, screen and remove iron from the slurry in the reactor to obtain a precursor.
[0046] In a third aspect, the present invention provides a lithium-rich manganese-based positive electrode material, wherein the raw materials for preparing the lithium-rich manganese-based positive electrode material include the lithium-rich manganese-based precursor described in the first aspect, or the lithium-rich manganese-based precursor prepared by the method described in the second aspect.
[0047] Preferably, the chemical formula of the lithium-rich manganese-based positive electrode material is Li 1.2 Ni x′ Mn y′ Nb a′ Co b′O2, wherein 0.25<x′≤0.4, 0.6≤y′<0.75, 0.001≤a′<0.005, 0.005≤b′<0.01, and x′+y′+a′+b′=1, the content of the Nb element decreases gradually from the inside to the outside, and the content of the Co element increases gradually from the inside to the outside, and the structure of the lithium-rich manganese-based positive electrode material is compact inside and loose outside.
[0048] Preferably, the outer surface of the lithium-rich manganese-based positive electrode material is coated with a coating layer, and the coating layer includes lithium cobalt oxide.
[0049] The lithium-rich manganese-based positive electrode material provided by the present invention has a gradient doping structure of Nb and Co and a structural feature of tight inside and loose outside, wherein Nb doping can increase the Li + The diffusion rate can be increased and the material structure can be stabilized, thereby improving the rate and cycle performance. Co doping can also stabilize the structure and improve the cycle performance. The compactness of the internal material can increase the density, thereby increasing the volume energy density, while the looseness of the external material can increase the contact area with the solid electrolyte and improve the rate performance.
[0050] The present invention does not specifically limit the preparation method of the lithium-rich manganese-based positive electrode material. By way of example and not limitation, the preparation method of the lithium-rich manganese-based positive electrode material comprises the following steps:
[0051] According to the molar ratio of lithium to the lithium-rich manganese-based precursor of 1.15-1.25 (for example, it can be 1.15, 1.17, 1.18, 1.19, 1.20, 1.22, 1.24 or 1.25, etc.), the lithium source and the lithium-rich manganese-based precursor material are evenly mixed, and sintered at a sintering temperature of 800°C-950°C for 10h-20h to obtain a lithium-rich manganese-based positive electrode material.
[0052] In this preferred technical solution, the sintering temperature is 800°C-950°C, for example, it can be 800°C, 820°C, 850°C, 870°C, 880°C, 900°C, 915°C, 930°C, 940°C or 950°C.
[0053] In this preferred technical solution, the sintering time is 10 h to 20 h, for example, it can be 10 h, 12 h, 15 h, 16 h, 17 h, 18 h, 19 h or 20 h.
[0054] Preferably, the lithium source comprises lithium carbonate and / or lithium hydroxide.
[0055] In a fourth aspect, the present invention provides a solid-state battery, comprising the lithium-rich manganese-based positive electrode material described in the third aspect.
[0056] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] (1) The lithium-rich manganese-based precursor of the present invention has a specific gradient doping structure and a tight inner and loose outer structure. The lithium-rich manganese-based positive electrode material prepared by using the precursor can inherit the gradient doping structure and the tight inner and loose outer structural characteristics of the precursor. Among them, Nb doping can improve Li + The diffusion rate can be increased and the material structure can be stabilized, thereby improving the rate and cycle performance. Co doping can also stabilize the structure and improve the cycle performance. The compactness of the internal material can increase the density, thereby increasing the volume energy density, while the looseness of the external material can increase the contact area with the solid electrolyte and improve the rate performance.
[0059] (2) The method of the present invention is simple and has good controllability. The element doping effect in the prepared lithium-rich manganese-based precursor is controllable, and the lithium-rich manganese-based positive electrode material prepared by the method has good performance. DETAILED DESCRIPTION
[0060] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0061] In the embodiments of the present invention, the molar ratio of nickel to manganese is 30:70, but it does not mean that it is only applicable to the preparation of precursors satisfying this molar ratio, and other molar ratios are also applicable to the present invention.
[0062] Example 1
[0063] This embodiment provides a lithium-rich manganese-based precursor for solid-state batteries (particle size D50 is 3 μm), and the chemical formula of the lithium-rich manganese-based precursor is Ni 0.297 Mn 0.693 Nb 0.001 Co 0.009 (OH)2, the content of Nb element decreases gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside. The structure of the lithium-rich manganese-based precursor is compact inside and loose outside. The outer surface of the lithium-rich manganese-based precursor is coated with a cobalt hydroxide coating layer, and the thickness of the coating layer is 0.1μm.
[0064] This embodiment also provides a method for preparing the above-mentioned lithium-rich manganese-based precursor, comprising the following steps:
[0065] Step 1, prepare a nickel-manganese salt solution with a metal concentration of 2 mol / L (wherein the nickel and manganese both come from sulfate) at a molar ratio of Ni:Mn=30:70; prepare a 1 g / L Nb salt solution (wherein the Nb comes from sulfate) and a 2 g / L Co salt solution (wherein the Co comes from sulfate), and adjust the pH values of the Nb salt solution and the Co salt solution to 2.0 with dilute sulfuric acid.
[0066] Step 2: Under a nitrogen atmosphere, nickel manganese salt solution, Nb salt solution, Co salt solution, sodium hydroxide solution and ammonia solution are added to the reactor in parallel, wherein the amount of Nb salt solution is fixed, and the Co salt solution is added to the Nb salt solution at a rate of 0.5 L / h. The two are mixed to form a mixed solution and then passed into the reactor.
[0067] Step 3, the temperature of the reactor is controlled at 40°C throughout the reaction. In the early stage of the reaction, the speed of the reactor is controlled at 500rpm, the pH is controlled at 11.8-12.0, and the ammonia concentration is controlled at 3.0g / L. When the precursor particle size grows to 2.5μm, the speed of the reactor is reduced to 300rpm, and the complexing agent is replaced with a sodium citrate solution. The concentration of sodium citrate is controlled at 0.2g / L. When the precursor particle size grows to 3.0μm, only 10g / L of Co salt solution, sodium hydroxide solution and sodium citrate solution are retained, and the feeding of other solutions is stopped, and the feeding flow rates of sodium hydroxide solution and citric acid solution are adjusted to keep the pH value and complexing agent concentration stable. Feeding is stopped after 18h of reaction.
[0068] Step 4: Wash, dry, screen and remove iron from the slurry in the reaction kettle to obtain a lithium-rich manganese-based precursor.
[0069] This embodiment also provides a lithium-rich manganese-based positive electrode material, the outer surface of the lithium-rich manganese-based positive electrode material is coated with a lithium cobalt oxide coating layer, and the chemical formula of the lithium-rich manganese-based positive electrode material (excluding the coating layer) is Li 1.2 Ni 0.297 Mn 0.693 Nb 0.001 Co 0.009 The contents of O2 and Nb elements decrease gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside. The structure of the lithium-rich manganese-based positive electrode material is compact inside and loose outside.
[0070] This embodiment also provides a method for preparing the above-mentioned lithium-rich manganese-based positive electrode material, comprising the following steps:
[0071] According to the molar ratio of lithium to lithium-rich manganese-based precursor being 1.2, lithium carbonate and the above-mentioned lithium-rich manganese-based precursor were evenly mixed, and sintered at 900° C. for 18 hours to obtain a lithium-rich manganese-based positive electrode material.
[0072] Example 2
[0073] This embodiment provides a lithium-rich manganese-based precursor for solid-state batteries (particle size D50 is 3.5 μm), the chemical formula of the lithium-rich manganese-based precursor is Ni 0.297 Mn 0.693 Nb 0.004 Co 0.006 (OH)2, the content of Nb element decreases gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside. The structure of the lithium-rich manganese-based precursor is compact inside and loose outside. The outer surface of the lithium-rich manganese-based precursor is coated with a cobalt hydroxide coating layer, and the thickness of the coating layer is 0.05μm.
[0074] This embodiment also provides a method for preparing the above-mentioned lithium-rich manganese-based precursor, comprising the following steps:
[0075] Step 1, prepare a nickel-manganese salt solution with a metal concentration of 3 mol / L (wherein the nickel and manganese both come from sulfate) at a molar ratio of Ni:Mn=30:70; prepare a 2 g / L Nb salt solution (wherein the Nb comes from sulfate) and a 3 g / L Co salt solution (wherein the Co comes from sulfate), and adjust the pH values of the Nb salt solution and the Co salt solution to 3.0 with dilute sulfuric acid.
[0076] Step 2: Under a helium atmosphere, nickel manganese salt solution, Nb salt solution, Co salt solution, sodium hydroxide solution and ammonia solution are added to the reactor in parallel, wherein the amount of Nb salt solution is fixed, and the Co salt solution is added to the Nb salt solution at a rate of 0.2 L / h. The two are mixed to form a mixed solution and then introduced into the reactor.
[0077] Step 3, the temperature of the reactor is controlled at 70°C throughout the reaction. In the early stage of the reaction, the speed of the reactor is controlled at 400rpm, the pH is controlled at 11.2-11.5, and the ammonia concentration is controlled at 8.0g / L. When the precursor particle size grows to 2.5μm, the speed of the reactor is reduced to 200rpm, and the complexing agent is replaced with a sodium citrate solution. The concentration of sodium citrate is controlled at 1g / L. When the precursor particle size grows to 3.5μm, only the Co salt solution, sodium hydroxide solution and sodium citrate solution are retained, and the feeding of other solutions is stopped, and the feeding flow rates of the sodium hydroxide solution and the citric acid solution are adjusted to keep the pH value and the concentration of the complexing agent stable. The feeding is stopped after the reaction for 10h.
[0078] Step 4: Wash, dry, screen and remove iron from the slurry in the reaction kettle to obtain a lithium-rich manganese-based precursor.
[0079] This embodiment also provides a lithium-rich manganese-based positive electrode material, the outer surface of the lithium-rich manganese-based positive electrode material is coated with a lithium cobalt oxide coating layer, and the chemical formula of the lithium-rich manganese-based positive electrode material is (excluding the coating layer) Li 1.2 Ni 0.297 Mn0.693 Nb 0.004 Co 0.006 The contents of O2 and Nb elements decrease gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside. The structure of the lithium-rich manganese-based positive electrode material is compact inside and loose outside.
[0080] This embodiment also provides a method for preparing the above-mentioned lithium-rich manganese-based positive electrode material, comprising the following steps:
[0081] According to the molar ratio of lithium to lithium-rich manganese-based precursor being 1.22, lithium carbonate and the above-mentioned lithium-rich manganese-based precursor were evenly mixed, and sintered at 800° C. for 20 hours to obtain a lithium-rich manganese-based positive electrode material.
[0082] Example 3
[0083] This embodiment provides a lithium-rich manganese-based precursor for solid-state batteries (particle size D50 is 3.2 μm), and the chemical formula of the lithium-rich manganese-based precursor is Ni 0.297 Mn 0.693 Nb 0.003 Co 0.007 (OH)2, the content of Nb element decreases gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside. The structure of the lithium-rich manganese-based precursor is compact inside and loose outside. The outer surface of the lithium-rich manganese-based precursor is coated with a cobalt hydroxide coating layer, and the thickness of the coating layer is 0.06μm.
[0084] This embodiment also provides a method for preparing the above-mentioned lithium-rich manganese-based precursor, comprising the following steps:
[0085] Step 1, prepare a nickel-manganese salt solution with a metal concentration of 1 mol / L (wherein the nickel and manganese both come from sulfate) at a molar ratio of Ni:Mn=30:70; prepare a 3 g / L Nb salt solution (wherein the Nb comes from sulfate) and a 5 g / L Co salt solution (wherein the Co comes from sulfate), and adjust the pH values of the Nb salt solution and the Co salt solution to 2.5 with dilute sulfuric acid.
[0086] Step 2: Under a nitrogen atmosphere, nickel manganese salt solution, Nb salt solution, Co salt solution, sodium hydroxide solution and ammonia solution are added to the reactor in parallel, wherein the amount of Nb salt solution is fixed, and the Co salt solution is added to the Nb salt solution at a rate of 1 L / h. The two are mixed to form a mixed solution and then passed into the reactor.
[0087] Step 3, the temperature of the reactor is controlled at 55°C throughout the reaction. In the early stage of the reaction, the speed of the reactor is controlled at 450rpm, the pH is controlled at 11.4-11.6, and the ammonia concentration is controlled at 5.0g / L. When the precursor particle size grows to 2.3μm, the speed of the reactor is reduced to 250rpm, and the complexing agent is replaced with a sodium citrate solution. The concentration of sodium citrate is controlled at 1.5g / L. When the precursor particle size grows to 3.2μm, only the Co salt solution, sodium hydroxide solution and sodium citrate solution are retained, and the feeding of other solutions is stopped, and the feeding flow rates of the sodium hydroxide solution and the citric acid solution are adjusted to keep the pH value and the concentration of the complexing agent stable. The feeding is stopped after the reaction for 15h.
[0088] Step 4: Wash, dry, screen and remove iron from the slurry in the reaction kettle to obtain a lithium-rich manganese-based precursor.
[0089] This embodiment also provides a lithium-rich manganese-based positive electrode material, the outer surface of the lithium-rich manganese-based positive electrode material is coated with a lithium cobalt oxide coating layer, and the chemical formula of the lithium-rich manganese-based positive electrode material is (excluding the coating layer) Li 1.2 Ni 0.297 Mn 0.693 Nb 0.003 Co 0.007 The contents of O2 and Nb elements decrease gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside. The structure of the lithium-rich manganese-based positive electrode material is compact inside and loose outside.
[0090] This embodiment also provides a method for preparing the above-mentioned lithium-rich manganese-based positive electrode material, comprising the following steps:
[0091] According to the molar ratio of lithium to lithium-rich manganese-based precursor being 1.25, lithium carbonate and the above-mentioned lithium-rich manganese-based precursor were evenly mixed, and sintered at 950° C. for 10 hours to obtain a lithium-rich manganese-based positive electrode material.
[0092] Example 4
[0093] The difference between this embodiment and embodiment 1 is that in step 3, in the early stage of the reaction, the speed of the reactor is controlled at 300 rpm, and when the precursor particle size grows to 2.5 μm, the speed of the reactor is increased to 500 rpm.
[0094] Example 5
[0095] The difference between this embodiment and embodiment 1 is that in step 3, the complexing agent is not replaced, ammonia water is used as the complexing agent throughout the whole process, and the ammonia concentration is controlled at 3.0 g / L.
[0096] Example 6
[0097] The difference between this embodiment and embodiment 1 is that in step 1, dilute sulfuric acid is not used to adjust the pH values of the Nb salt solution and the Co salt solution. In this embodiment, the pH values of the Nb salt solution and the Co salt solution are 4 and 3.5, respectively.
[0098] Example 7
[0099] The difference between this embodiment and embodiment 1 is that in step 3, when the particle size of the precursor grows to 3.0 μm, the concentration of the Co salt solution is 100 g / L, and the reaction time is continued for 1.8 h.
[0100] Comparative Example 1
[0101] The difference between this comparative example and Example 1 is that in step 2, the Co salt solution is not added to the Nb salt solution at a rate of 0.5 L / h.
[0102] Comparative Example 2
[0103] The difference between this comparative example and Example 1 is that the rotation speed and the complexing agent remain unchanged, so that the internal and external structures of the precursor are relatively compact.
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 1 is that the chemical formula of the lithium-rich manganese-based precursor is Ni 0.297 Mn 0.693 Nb 0.01 Co 0.009 (OH)2.
[0106] Comparative Example 4
[0107] The difference between this comparative example and Example 1 is that the chemical formula of the lithium-rich manganese-based precursor is Ni 0.297 Mn 0.693 Nb 0.001 Co 0.02 (OH)2.
[0108] Battery preparation:
[0109] Positive electrode preparation: Mix and grind the lithium-rich manganese-based positive electrode material, solid electrolyte Li3InCl6, and conductive agent Super P in a mass ratio of 5:4:1.
[0110] Battery assembly: Use the above mixture as the positive electrode material, Li3InCl6 as the solid electrolyte, and lithium indium alloy as the negative electrode to assemble into a solid-state battery.
[0111] Performance Testing:
[0112] (1) Rate performance test: 25°C, 2.0-4.8V, 8C / 0.5C discharge capacity ratio.
[0113] (2) Cycle performance test: Capacity retention rate after 1000 cycles at 25°C, 2.0-4.8V, 0.5C.
[0114] The results are shown in Table 1.
[0115] Table 1
[0116] Rate performance (%) Cycle performance (%) Example 1 90.2 98.9 Example 2 90.5 99.0 Example 3 90.3 98.7 Example 4 87.2 95.3 Example 5 85.4 90.1 Example 6 85.7 86.2 Example 7 88.2 96.1 Comparative Example 1 80.1 82.4 Comparative Example 2 70.7 79.3 Comparative Example 3 90.1 98.7 Comparative Example 4 90.0 98.8
[0117] As can be seen from Table 1, the preparation method of the ternary precursor provided by the present invention is simple, and the rate performance and cycle performance of the positive electrode material prepared therefrom can be effectively improved by gradient doping with Nb and Co and regulating the morphology of the precursor.
[0118] By comparing Example 1 with Example 4, it can be seen that increasing the rotation speed in the later stage of the reaction will cause the looseness of the material's external structure to decrease, and the rate and cycle performance to decrease.
[0119] By comparing Example 1 with Example 5, it can be seen that ammonia water is used as a complexing agent throughout the process, the external structure of the material is not loose enough, and the rate and cycle performance are reduced.
[0120] By comparing Example 1 with Example 6, it can be seen that the different pH values of the doping solutions will cause pH fluctuations in the mixed solution. The large pH fluctuations during the reaction process will lead to the generation of fine powders, which will have a particularly large impact on the cycle performance.
[0121] By comparing Example 1 with Example 7, it can be seen that increasing the concentration of the Co salt solution during the coating stage and keeping the time too short will cause incomplete coating on the surface of many particles, thus reducing the coating effect.
[0122] By comparing Example 1 with Comparative Example 1, it can be seen that the gradient doping of Co element can effectively improve the rate and cycle performance of the material.
[0123] By comparing Example 1 with Comparative Example 2, it can be seen that the structure of the material has a significant impact on the rate and cycle performance, and a loose structure is conducive to the performance of the rate and cycle performance.
[0124] By comparing Example 1 with Comparative Example 3, it can be seen that further increasing the Nb doping amount will not further improve the performance, but the Nb element is expensive and the cost increases significantly.
[0125] By comparing Example 1 with Comparative Example 4, it can be seen that further increasing the Co element has no effect on improving the performance, but will increase the cost of raw materials.
[0126] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A lithium-rich manganese-based precursor for solid-state batteries, characterized in that: The chemical formula of the lithium-rich manganese-based precursor is Ni x Mn y Nb a Co b (OH)2, wherein 0.25<x≤0.4, 0.6≤y<0.75, 0.001≤a<0.005, 0.005≤b<0.01, and x+y+a+b=1, the content of Nb element decreases gradually from the inside to the outside, and the content of Co element increases gradually from the inside to the outside, and the structure of the lithium-rich manganese-based precursor is compact inside and loose outside.
2. The lithium-rich manganese-based precursor according to claim 1, characterized in that: The particle size D50 of the lithium-rich manganese-based precursor is 3 μm-3.5 μm.
3. The lithium-rich manganese-based precursor according to claim 1 or 2, characterized in that: The outer surface of the lithium-rich manganese-based precursor is coated with a coating layer, and the coating layer includes cobalt hydroxide; Preferably, the coating layer has a thickness of 0.05 μm-0.1 μm.
4. A method for preparing a lithium-rich manganese-based precursor according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: A coprecipitation reaction is carried out using a nickel-manganese salt solution, a Nb salt solution, a Co salt solution, a precipitant solution and a complexing agent solution. During the reaction, the content of the Nb element provided by the Nb salt solution and the Co salt solution is controlled to gradually decrease while the content of the Co element is gradually increased.
5. The method for preparing a lithium-rich manganese-based precursor according to claim 4, characterized in that: The temperature of the coprecipitation reaction is 40°C-80°C; Preferably, the coprecipitation reaction is carried out under the protection of a protective gas; Preferably, the protective gas includes at least one of nitrogen, helium and argon.
6. The method for preparing a lithium-rich manganese-based precursor according to claim 4 or 5, characterized in that: The reaction is divided into an early reaction stage and a late reaction stage. The early reaction stage is the stage from the generation of the precursor to the growth to a particle size of D = (70% - 85%) × D0, wherein D0 is the target particle size; Preferably, in the early stage of the reaction, the rotation speed of the coprecipitation reaction is 400rpm-500rpm; Preferably, in the early stage of the reaction, the pH value of the coprecipitation reaction is 11.0-12.0; Preferably, in the early stage of the reaction, the complexing agent is aqueous ammonia; Preferably, in the early stage of the reaction, the ammonia concentration in the reaction system is 3.0 g / L-10.0 g / L; Preferably, in the later stage of the reaction, the rotation speed of the coprecipitation reaction is 200rpm-300rpm; Preferably, in the later stage of the reaction, the complexing agent is a sodium citrate solution; Preferably, in the later stage of the reaction, the concentration of sodium citrate in the reaction system is 0.2 g / L-2 g / L.
7. The method for preparing a lithium-rich manganese-based precursor according to any one of claims 4 to 6, characterized in that: The method of controlling the Nb salt solution and the Co salt solution to gradually reduce the content of the Nb element and gradually increase the content of the Co element is: Adding nickel-manganese salt solution, Nb salt solution, Co salt solution, precipitant solution and complexing agent solution into a reaction kettle in parallel, wherein the amount of Nb salt solution is fixed, and the Co salt solution is added to the Nb salt solution at a certain rate; Preferably, the certain rate is 0.1L / h-1L / h; Preferably, the pH value of the Nb salt solution and the Co salt solution is the same.
8. The method for preparing a lithium-rich manganese-based precursor according to any one of claims 4 to 7, characterized in that: The method further comprises coating the precursor when the precursor grows to a particle size D0, wherein the coating method is: stopping the use of the Nb salt solution and only retaining the nickel manganese salt solution, the Co salt solution, the precipitant solution and the complexing agent solution for coprecipitation reaction; Preferably, in the coating method, the pH value and the complexing agent concentration are stabilized by adjusting the strength of the precipitant solution and the complexing agent solution; Preferably, in the coating method, the concentration of the Co salt solution is 1 g / L-10 g / L; Preferably, in the coating method, the coprecipitation reaction time is 10h-20h.
9. A lithium-rich manganese-based positive electrode material, characterized in that: The raw material for preparing the lithium-rich manganese-based positive electrode material includes the lithium-rich manganese-based precursor according to any one of claims 1 to 3, or the lithium-rich manganese-based precursor prepared by the method according to any one of claims 4 to 8; Preferably, the chemical formula of the lithium-rich manganese-based positive electrode material is Li 1.2 Ni x′ Mn y′ Nb a′ Co b′ O2, wherein 0.25<x′≤0.4, 0.6≤y′<0.75, 0.001≤a′<0.005, 0.005≤b′<0.01, and x′+y′+a′+b′=1, the content of the Nb element decreases from the inside to the outside, and the content of the Co element increases from the inside to the outside, and the structure of the lithium-rich manganese-based positive electrode material is compact inside and loose outside; Preferably, the outer surface of the lithium-rich manganese-based positive electrode material is coated with a coating layer, and the coating layer includes lithium cobalt oxide.
10. A solid-state battery, characterized in that: The solid-state battery comprises the lithium-rich manganese-based positive electrode material according to claim 9.
Citation Information
Cited By
Double-gradient positive electrode precursor material and preparation method and application thereof
CN119330425A
Micro-nano magnesium-doped indium-coated lithium-rich manganese-based positive electrode material and precursor and preparation method thereof
CN119349666A
High-nickel ternary material with gradient doping of high-valence elements, preparation method of high-nickel ternary material and solid-state battery
CN121528888A