NiO-Co3O4 composite material as well as preparation method and application thereof

By preparing NiO-Co3O4 composite material and utilizing its high specific surface area and honeycomb structure, the problem of insufficient hydrogen sulfide detection sensitivity and selectivity in the existing technology is solved, and an efficient and low-power hydrogen sulfide gas sensor is realized.

CN118724089APending Publication Date: 2024-10-01GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410784133.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing semiconductor gas sensors based on metal oxides have insufficient sensitivity, poor selectivity, and high operating temperatures in hydrogen sulfide detection, resulting in high power consumption and difficulty in meeting accuracy requirements.

Method used

Using NiO-Co3O4 composite material, through co-precipitation reaction and adding acetic acid as a structural directing agent, a honeycomb NiO-Co3O4 composite material with a specific surface area greater than 20m2/g is prepared, which is used to prepare gas-sensitive materials and sensors and improves the resistance to hydrogen sulfide. Detection sensitivity and selectivity.

Benefits of technology

It achieves high sensitivity, fast response, low power consumption and good selectivity to hydrogen sulfide gas, and is suitable for low-concentration hydrogen sulfide detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724089A_ABST
    Figure CN118724089A_ABST
Patent Text Reader

Abstract

The invention discloses a NiO-Co3O4 composite material as well as a preparation method and application thereof, and belongs to the technical field of sensor materials. The composite material is honeycomb-shaped; and the specific surface area is not less than 20m < 2 > / g. The composite material has a relatively large specific surface area, and is beneficial to improving the sensitivity of the gas sensitive material. The preparation method comprises the following steps: carrying out a co-precipitation reaction on a mixed solution containing cobalt salt, nickel salt and a structure-directing agent and a precipitant solution until the cobalt nickel carbonate material with a target particle size is obtained; and calcining the cobalt nickel carbonate material. Wherein the structure-directing agent is acetic acid. The preparation method is simple and easy to operate, the honeycomb-shaped composite material with the large specific surface area can be obtained, acetic acid is free of residues after being calcined, and adverse effects on the gas sensitivity of the material are avoided. The composite material can be used as a gas sensitive material for preparing a sensor, is especially suitable for detecting hydrogen sulfide gas, and has the advantages of high sensitivity, good selectivity, low power consumption and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sensor materials, and in particular to a NiO-Co3O4 composite material and a preparation method and application thereof. Background Art

[0002] Hydrogen sulfide is a highly toxic substance and a byproduct of many industrial processes, such as natural gas refining, oil refining, wastewater treatment and papermaking. Even dilute hydrogen sulfide has an impact on the eyes, respiratory system and central nervous system. Inhaling a small amount of high-concentration hydrogen sulfide can be fatal in a short period of time. Therefore, the detection of low-concentration hydrogen sulfide is of great significance and value to protecting health and improving the quality of life.

[0003] Among various gas detection technologies, gas sensors based on semiconductor oxides have become a cutting-edge research hotspot due to their advantages such as small size, high reliability, rapid response and easy integration.

[0004] In the existing technology, common metal oxide-based semiconductor gas sensors and electrochemical sensors still have many problems to be solved, such as insufficient sensitivity, poor selectivity, high operating temperature resulting in high power consumption, and other practical problems, which often fail to meet the accuracy requirements for hydrogen sulfide detection.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a NiO-Co3O4 composite material and a preparation method and application thereof, so as to solve or improve the above technical problems.

[0007] The present invention can be implemented like this:

[0008] In a first aspect, the present invention provides a NiO-Co3O4 composite material, wherein the NiO-Co3O4 composite material is honeycomb-shaped; and the specific surface area of ​​the NiO-Co3O4 composite material is not less than 20m 2 / g.

[0009] In an optional embodiment, the NiO-Co3O4 composite material is a composite material of NiO and NiCo2O4.

[0010] In a second aspect, the present invention provides a method for preparing a NiO-Co3O4 composite material as described in the above embodiment, comprising the following steps: coprecipitating a mixed solution containing a cobalt salt, a nickel salt and a structure directing agent with a precipitant solution for providing carbonate ions until a nickel cobalt carbonate material having a target particle size is obtained; calcining the nickel cobalt carbonate material;

[0011] Wherein, the structure directing agent is acetic acid.

[0012] In an optional embodiment, the preparation of the nickel cobalt carbonate material has at least one of the following characteristics:

[0013] Feature 1: The cobalt salt includes at least one of cobalt chloride, cobalt sulfate and cobalt nitrate;

[0014] Feature 2: The nickel salt includes at least one of nickel chloride, nickel sulfate and nickel nitrate;

[0015] Feature 3: The precipitant includes at least one of ammonium bicarbonate, ammonium carbonate and sodium carbonate;

[0016] Feature 4: The concentration of cobalt salt in the mixed solution is 50 g / L to 80 g / L;

[0017] Feature 5: The concentration of nickel salt in the mixed solution is 50 g / L to 80 g / L;

[0018] Feature 6: The concentration of the structure directing agent in the mixed solution is 0.1 g / L to 1 g / L;

[0019] Feature 7: The pH of the coprecipitation reaction is 6 to 8;

[0020] Feature 8: The coprecipitation reaction is carried out under stirring conditions; preferably, the stirring speed is 200r / min to 500r / min;

[0021] Feature 9: The target particle size of the nickel cobalt carbonate material is not less than 1 μm, preferably 1 μm to 5 μm.

[0022] In an optional embodiment, the mixed solution and the precipitant solution are simultaneously fed into a reaction device having a base liquid to perform a co-precipitation reaction.

[0023] In an optional embodiment, the base liquid has at least one of the following characteristics:

[0024] Feature 10: The base liquid is a solution containing carbonate ions; preferably, the base liquid is an aqueous solution of ammonium bicarbonate; preferably, in the aqueous solution of ammonium bicarbonate, 0.005 kg to 0.01 kg of ammonium bicarbonate is added per liter of water;

[0025] Feature 11: The temperature of the base liquid is 30°C to 40°C.

[0026] In an optional embodiment, the calcination has at least one of the following characteristics:

[0027] Feature 12: The calcination temperature is 400°C to 700°C;

[0028] Feature 13: Calcination time is 1h to 6h;

[0029] Feature 14: The heating rate of the calcination process is 2°C / min to 8°C / min.

[0030] In an optional embodiment, before calcining, the nickel cobalt carbonate material is further washed and dried.

[0031] In an optional embodiment, the drying temperature is 100°C to 120°C.

[0032] In an optional embodiment, the drying time is 16 hours to 20 hours.

[0033] In a third aspect, the present invention provides a gas-sensitive material, which includes the NiO-Co3O4 composite material of the aforementioned embodiment.

[0034] In a fourth aspect, the present invention provides a sensor, wherein the gas-sensitive material of the sensor includes the gas-sensitive material of the aforementioned embodiment.

[0035] In an alternative embodiment, the sensor is a gas sensor.

[0036] In an optional embodiment, the sensor includes a ceramic member, and a surface of the ceramic member has an active layer formed of a gas-sensitive material.

[0037] In an optional embodiment, the thickness of the active layer is 10 μm to 40 μm.

[0038] In a fifth aspect, the present invention provides a use of a NiO-Co3O4 composite material as described in the aforementioned embodiment, or a gas-sensitive material as described in the aforementioned embodiment, or a sensor as described in any one of the aforementioned embodiments in detecting hydrogen sulfide gas.

[0039] The beneficial effects of the present invention include:

[0040] The present invention adds a specific structure-directing agent, acetic acid, so that the prepared NiO-Co3O4 composite material is honeycomb-shaped and has a large specific surface area, which can provide more active sites for gas adsorption, and is conducive to increasing the sensitivity of the NiO-Co3O4 composite material; and the acetic acid has no residue after calcination, avoiding adverse effects on the gas sensitivity of the material. The preparation method of the NiO-Co3O4 composite material is simple, easy to operate, and can be industrially produced. The composite material can be used as a gas-sensitive material to prepare a sensor, which is particularly suitable for detecting hydrogen sulfide gas, and has the advantages of high sensitivity, fast response, good selectivity, good stability, low power consumption, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0042] Figure 1 This is a SEM image of the NiO-Co3O4 composite material prepared in Example 1 of the present invention;

[0043] Figure 2 This is a SEM image of the NiO-Co3O4 composite material prepared in Example 2 of the present invention;

[0044] Figure 3 This is a SEM image of the NiO-Co3O4 composite material prepared in Example 3 of the present invention;

[0045] Figure 4 This is the XRD pattern of the NiO-Co3O4 composite material prepared in Example 3 of the present invention;

[0046] Figure 5 This is a SEM image of the NiO-Co3O4 composite material prepared in Example 4 of the present invention;

[0047] Figure 6 This is a SEM image of the NiO-Co3O4 composite material prepared in Comparative Example 1 of the present invention;

[0048] Figure 7 This is a SEM image of the NiO-Co3O4 composite material prepared in Comparative Example 2 of the present invention;

[0049] Figure 8 It is a dot-line graph of the sensitivity of the gas sensors prepared in Examples 1 to 3 and Comparative Example 1 in the test example to 10 ppm hydrogen sulfide gas at different temperatures;

[0050] Fig. 9 The graph is a response curve of the gas sensor prepared in Example 3 of the test example to hydrogen sulfide gas of different concentrations at 80°C;

[0051] Fig.10 This is a graph showing the selectivity results of the gas sensor prepared in Example 3 of the experimental example for different gases. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0053] The NiO-Co3O4 composite material provided by the present invention and its preparation method and application are specifically described below.

[0054] The present invention provides a NiO-Co3O4 composite material, which is in a honeycomb shape; and the specific surface area of ​​the NiO-Co3O4 composite material is not less than 20m 2 / g.

[0055] The above-mentioned "NiO-Co3O4 composite material" refers to a composite material of NiO and NiCo2O4. Specifically, the Co in the composite material Co3O4 2+ Partial Ni 2+ Replaced to form NiCo2O4, and some Ni 2+ Exists in the form of NiO.

[0056] In some optional embodiments, the specific surface area of ​​the NiO-Co3O4 composite material can be 21.3 m 2 / g~46.2m 2 / g, such as 21.3m 2 / g, 32.5m 2 / g or 46.2m 2 / g, etc., can also be 21.3m 2 / g~46.2m 2 / Other values ​​within the range of g.

[0057] The present invention creatively provides a honeycomb-shaped NiO-Co3O4 composite material structure, which has a large specific surface area and can provide more active sites for gas adsorption, which is beneficial to improving the sensitivity and selectivity of gas (especially hydrogen sulfide gas) detection.

[0058] Accordingly, the present invention provides a method for preparing the above-mentioned NiO-Co3O4 composite material, comprising the following steps: coprecipitating a mixed solution containing a cobalt salt, a nickel salt and a structure directing agent with a precipitant solution for providing carbonate ions until a nickel cobalt carbonate material with a target particle size is obtained; calcining the nickel cobalt carbonate material;

[0059] Wherein, the structure directing agent is acetic acid.

[0060] In some embodiments, a mixed solution and a precipitant solution are simultaneously added into a reaction device having a base solution to perform a co-precipitation reaction.

[0061] The reaction device may be a reactor, and the volume of the reactor may be 5L to 500L by way of example but not limitation.

[0062] The bottom liquid is a solution containing carbonate ions. For example, the bottom liquid can be at least one of an aqueous solution of ammonium bicarbonate, an aqueous solution of ammonium carbonate, and an aqueous solution of sodium carbonate. In some preferred embodiments, the bottom liquid is of the same type as the precipitant solution. The volume of the bottom liquid can be, for example, half the volume of the reaction device. Taking the bottom liquid as an aqueous solution of ammonium bicarbonate as an example, in the aqueous solution of ammonium bicarbonate, 0.005kg to 0.01kg (such as 0.005kg, 0.006kg, 0.007kg, 0.008kg, 0.009kg or 0.01kg, etc.) of ammonium bicarbonate can be added per liter of water.

[0063] The temperature of the base liquid can be 30°C to 40°C, such as 30°C, 32°C, 35°C, 38°C or 40°C, etc., or other values ​​within the range of 30°C to 40°C.

[0064] After adding the base liquid into the reaction container, stirring can be started, and the stirring speed can be 200r / min to 500r / min, such as 200r / min, 300r / min, 400r / min or 500r / min.

[0065] In some optional embodiments, the cobalt salt may illustratively but not limitatively include at least one of cobalt chloride, cobalt sulfate and cobalt nitrate.

[0066] The nickel salt may illustratively but not limitatively include at least one of nickel chloride, nickel sulfate, and nickel nitrate.

[0067] The precipitating agent may illustratively but not limitatively include at least one of ammonium bicarbonate, ammonium carbonate, and sodium carbonate.

[0068] In some optional embodiments, the concentration of cobalt salt in the mixed solution can be 50g / L to 80g / L, such as 50g / L, 55g / L, 60g / L, 65g / L, 70g / L, 75g / L or 80g / L, etc., or it can be other values ​​within the range of 50g / L to 80g / L.

[0069] The concentration of nickel salt in the mixed solution may also be 50 g / L to 80 g / L, such as 50 g / L, 55 g / L, 60 g / L, 65 g / L, 70 g / L, 75 g / L or 80 g / L, or other values ​​within the range of 50 g / L to 80 g / L.

[0070] The concentration of the structure directing agent in the mixed solution can be 0.1g / L to 1g / L, such as 0.1g / L, 0.2g / L, 0.3g / L, 0.4g / L, 0.5g / L, 0.6g / L, 0.7g / L, 0.8g / L, 0.9g / L or 1g / L, etc., or it can be other values ​​within the range of 0.1g / L to 1g / L.

[0071] It should be emphasized that the inventor creatively discovered that, by specifically using acetic acid as a structure-directing agent, the carboxyl group in the acetic acid molecule has negative charge and can form coordination bonds with metal cations on the crystal surface, thereby adsorbing on the crystal surface. This adsorption can change the energy and active sites on the crystal surface, causing the crystal growth rate to change in a specific direction, thereby achieving a structure-directing effect. In addition, the methyl group in the acetic acid molecule can form a hydrophobic interaction with the crystal surface, thereby affecting the affinity of the crystal surface. This effect can increase or slow down the growth rate of the crystal in a specific direction, thereby controlling the growth direction and morphology of the crystal. Therefore, acetic acid can change the morphology of the material during the coprecipitation reaction, so that the composite material after calcination is finally honeycombed and has a large specific surface area. While using other conventional structure-directing agents, such as ammonia or monomethylamine, although the material can also be structure-directed to a certain extent, the composite material finally obtained is not honeycombed, and the specific surface area is small (such as less than 20m 2 / g). For example, when ammonia water is used as the structure directing agent, the NiO-Co3O4 composite material finally prepared has a solid sphere structure.

[0072] In addition, by using acetic acid as a structure directing agent, no residue will be produced after washing and calcination, thus avoiding the adverse effect of some acetic acid remaining inside the material on the gas-sensing properties of the material, which is beneficial to improving the sensitivity of the material.

[0073] The concentration of acetic acid will affect the structure of the composite material. As the concentration of acetic acid increases, during the coprecipitation process, the morphology of the primary particles gradually changes from flake to granular, and the secondary spheres change from intercalated flakes to densely packed structures, with the specific surface area gradually increasing. If the concentration of acetic acid is lower than 0.1 g / L, the morphology transformation cannot be completed; if the concentration of acetic acid exceeds 1 g / L, the primary particles will be extremely small and it will be difficult for the particles to form spheres.

[0074] In some optional embodiments, the pH of the coprecipitation reaction may be 6-8, such as 6, 6.5, 7, 7.5 or 8, or other values ​​within the range of 6-8.

[0075] If the pH value of the co-precipitation reaction is lower than 6, it is easy to cause precipitation to be difficult and the loss of cobalt and nickel is serious; if the pH value of the co-precipitation reaction is higher than 8, it is easy to cause particle agglomeration and severe agglomeration.

[0076] The coprecipitation reaction is carried out under stirring conditions. For example, the stirring speed may be 200 r / min to 500 r / min, such as 200 r / min, 300 r / min, 400 r / min or 500 r / min.

[0077] In some embodiments, the target particle size of the nickel cobalt carbonate material is not less than 1 μm, for example, it can be 1 μm to 5 μm, such as 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, etc., or other values ​​within the range of 1 μm to 5 μm.

[0078] If the target particle size of the nickel cobalt carbonate material is less than 1 μm, the sphericity of the nickel cobalt carbonate material will be poor; if the target particle size of the nickel cobalt carbonate material exceeds 5 μm, it will be unfavorable for the preparation of gas sensors.

[0079] In some specific operations, a mixed solution containing cobalt salt, nickel salt and structure directing agent and an ammonium bicarbonate solution are added to the bottom liquid in parallel, the flow rate of the ammonium bicarbonate solution is controlled, the reaction pH is maintained within a preset range (6 to 8), suction filtration is started after the kettle is full, and the liquid level in the reactor is maintained near the overflow port, and the particle size of the nickel cobalt carbonate material grows to the target particle size, and then the liquid addition is stopped to obtain a nickel cobalt carbonate slurry.

[0080] In some embodiments, the slurry containing the nickel cobalt carbonate material obtained from the co-precipitation reaction (ie, nickel cobalt carbonate slurry) is centrifuged, washed, and dried.

[0081] Wherein, washing can be carried out with pure water, and the volume of the pure water can be, for example, 0.5 to 1.5 times (such as 0.5 times, 1 times or 1.5 times, etc.) of the nickel cobalt carbonate slurry.

[0082] The drying temperature may be 100° C. to 120° C., such as 100° C., 105° C., 110° C., 115° C. or 120° C., or other values ​​within the range of 100° C. to 120° C. The drying time may be 16 h to 20 h, such as 16 h, 17 h, 18 h, 19 h or 20 h, or other values ​​within the range of 16 h to 20 h.

[0083] If the drying temperature exceeds 120°C, nickel cobalt carbonate is prone to decomposition and oxidation.

[0084] The drying process can be performed in a vacuum oven or a nitrogen oven by way of example but not limitation.

[0085] In some embodiments, the calcination temperature may be 400°C to 700°C, such as 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C, or any other value within the range of 400°C to 700°C.

[0086] If the calcination temperature is lower than 400°C, it is not conducive to the complete oxidation of nickel cobalt carbonate; if the calcination temperature is higher than 700°C, it is easy to cause deformation or cracking of the particles.

[0087] The calcination time may be 1 h to 6 h, such as 1 h, 2 h, 3 h, 4 h, 5 h or 6 h, etc., or may be any other value within the range of 1 h to 6 h.

[0088] If the calcination time is shorter than 1 hour, it is not conducive to the complete oxidation of nickel cobalt carbonate; if the calcination time is longer than 6 hours, it is easy to cause particles to stick together and the dispersibility becomes poor.

[0089] The heating rate of the above calcination process can be 2°C / min to 8°C / min, such as 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min or 8°C / min, or other values ​​within the range of 2°C / min to 8°C / min.

[0090] If the heating rate is too fast, the material may crack; if the heating rate is too slow, the material may be difficult to burn through.

[0091] The calcination process can be performed, by way of example but not limitation, in a muffle furnace or a rotary kiln.

[0092] As mentioned above, the preparation method provided by the present invention is simple in process and easy to operate, and can obtain a NiO-Co3O4 composite material with a honeycomb shape and a large specific surface area.

[0093] In addition, the present invention also provides a gas-sensitive material, which includes the above-mentioned NiO-Co3O4 composite material.

[0094] The gas-sensitive material has high selectivity and sensitivity to hydrogen sulfide gas.

[0095] In addition, the present invention also provides a sensor, the gas-sensitive material of the sensor includes the above-mentioned gas-sensitive material.

[0096] In some embodiments, the sensor is a gas sensor, especially a gas sensor for detecting hydrogen sulfide gas, which has the advantages of high sensitivity, fast response and recovery time, good stability and good selectivity.

[0097] In some embodiments, the sensor includes a ceramic part, and the surface of the ceramic part has an active layer formed of the gas-sensitive material. Exemplarily, the thickness of the active layer can be 10 μm to 40 μm, such as 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm or 40 μm. The ceramic part can be a ceramic tube with two gold electrodes and four platinum wires, and the active layer completely covers the gold electrodes.

[0098] In some embodiments, the sensor can respond quickly to low concentrations of hydrogen sulfide at 80°C and has good selectivity.

[0099] Correspondingly, the present invention also provides the use of the above-mentioned NiO-Co3O4 composite material, gas-sensitive material and sensor in detecting hydrogen sulfide gas.

[0100] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0101] Example 1

[0102] This embodiment provides a gas sensor based on a NiO-Co3O4 composite material, and the preparation method thereof includes:

[0103] Step (1): add 250L of pure water to a 500L reactor until the reactor is half full, start stirring at a speed of 400r / min, heat the water to 37°C, and after the temperature in the reactor stabilizes, add 2kg of ammonium bicarbonate solid to the water in the reactor and mix well.

[0104] Step (2): After the bottom liquid environment is stable, add ammonium bicarbonate solution and a mixed solution formed by cobalt sulfate, nickel sulfate and acetic acid to the reactor in parallel, wherein the concentration of cobalt sulfate in the mixed solution is 60g / L of cobalt sulfate, the concentration of nickel sulfate in the mixed solution is 60g / L, the concentration of acetic acid in the mixed solution is 0.1g / L, and the flow rate of the mixed solution is 25L / h. Control the flow rate of the ammonium bicarbonate solution to keep the reaction pH at 7.5, start suction filtration after the kettle is full, keep the reactor liquid level near the overflow port, and stop feeding the liquid after the particle size of the nickel cobalt carbonate material grows to 4μm, to obtain nickel cobalt carbonate slurry (500L).

[0105] Step (3): centrifuge, wash and dry the nickel cobalt carbonate slurry. The washing water is 750L pure water, and the powder is dried in a blast oven at 110°C for 16 hours. The dried powder is calcined in a muffle furnace at a heating rate of 5°C / min, a calcination temperature of 600°C, and a holding time of 2 hours to obtain a honeycomb NiO-Co3O4 composite material.

[0106] Step (4): Grind and mix the prepared NiO-Co3O4 composite material with deionized water to form a viscous slurry; evenly apply the slurry on a ceramic tube with two gold electrodes and four platinum wires, and use the nickel-chromium alloy wire on the inside of the tube as a heating resistor of a side-heated heating device to obtain a working electrode; after drying the obtained working electrode in the shade overnight, place it in a muffle furnace and calcine it at 300°C for 30 minutes to obtain a gas sensor with stable performance.

[0107] Example 2

[0108] This embodiment provides a gas sensor based on a NiO-Co3O4 composite material, and the preparation method thereof includes:

[0109] Step (1): add 250L of pure water to a 500L reactor until the reactor is half full, start stirring at a speed of 400r / min, heat the water to 37°C, and after the temperature in the reactor stabilizes, add 2kg of ammonium bicarbonate solid to the water in the reactor and mix well.

[0110] Step (2): After the bottom liquid environment is stable, add ammonium bicarbonate solution and a mixed solution formed by cobalt sulfate, nickel sulfate and acetic acid to the reactor in parallel, wherein the concentration of cobalt sulfate in the mixed solution is 60g / L of cobalt sulfate, the concentration of nickel sulfate in the mixed solution is 60g / L, the concentration of acetic acid in the mixed solution is 0.5g / L, and the flow rate of the mixed solution is 25L / h. Control the flow rate of the ammonium bicarbonate solution to keep the reaction pH at 7.5, start suction filtration after the kettle is full, keep the reactor liquid level near the overflow port, and stop feeding the liquid after the particle size of the nickel cobalt carbonate material grows to 4μm, to obtain nickel cobalt carbonate slurry (500L).

[0111] Step (3): centrifuge, wash and dry the nickel cobalt carbonate slurry. The washing water is 750L pure water, and the powder is dried in a blast oven at 110°C for 16 hours. The dried powder is calcined in a muffle furnace at a heating rate of 5°C / min, a calcination temperature of 600°C, and a holding time of 2 hours to obtain a honeycomb NiO-Co3O4 composite material.

[0112] Step (4): Grind and mix the prepared NiO-Co3O4 composite material with deionized water to form a viscous slurry; evenly apply the slurry on a ceramic tube with two gold electrodes and four platinum wires, and use the nickel-chromium alloy wire on the inside of the tube as a heating resistor of a side-heated heating device to obtain a working electrode; after drying the obtained working electrode in the shade overnight, place it in a muffle furnace and calcine it at 300°C for 30 minutes to obtain a gas sensor with stable performance.

[0113] That is, the difference between this embodiment and embodiment 1 is that the concentration of acetic acid is different.

[0114] Example 3

[0115] This embodiment provides a gas sensor based on a NiO-Co3O4 composite material, and the preparation method thereof includes:

[0116] Step (1): add 250L of pure water to a 500L reactor until the reactor is half full, start stirring at a speed of 400r / min, heat the water to 37°C, and after the temperature in the reactor stabilizes, add 2kg of ammonium bicarbonate solid to the water in the reactor and mix well.

[0117] Step (2): After the bottom liquid environment is stable, add ammonium bicarbonate solution and a mixed solution formed by cobalt sulfate, nickel sulfate and acetic acid to the reactor in parallel, wherein the concentration of cobalt sulfate in the mixed solution is 60g / L of cobalt sulfate, the concentration of nickel sulfate in the mixed solution is 60g / L, the concentration of acetic acid in the mixed solution is 1g / L, and the flow rate of the mixed solution is 25L / h. Control the flow rate of the ammonium bicarbonate solution to keep the reaction pH at 7.5, start suction filtration after the kettle is full, keep the reactor liquid level near the overflow port, and stop feeding the liquid until the particle size of the nickel cobalt carbonate material grows to 4μm, and obtain nickel cobalt carbonate slurry (500L).

[0118] Step (3): centrifuge, wash and dry the nickel cobalt carbonate slurry. The washing water is 750L pure water, and the powder is dried in a blast oven at 110°C for 16 hours. The dried powder is calcined in a muffle furnace at a heating rate of 5°C / min, a calcination temperature of 600°C, and a holding time of 2 hours to obtain a honeycomb NiO-Co3O4 composite material.

[0119] Step (4): Grind and mix the prepared NiO-Co3O4 composite material with deionized water to form a viscous slurry; evenly apply the slurry on a ceramic tube with two gold electrodes and four platinum wires, and use the nickel-chromium alloy wire on the inside of the tube as a heating resistor of a side-heated heating device to obtain a working electrode; after drying the obtained working electrode in the shade overnight, place it in a muffle furnace and calcine it at 300°C for 30 minutes to obtain a gas sensor with stable performance.

[0120] That is, the difference between this embodiment and embodiment 1 is that the concentration of acetic acid is different.

[0121] Example 4

[0122] The difference between this embodiment and embodiment 1 is that the concentration of the structure directing agent acetic acid in the mixed solution is 2 g / L.

[0123] Example 5

[0124] This embodiment provides a gas sensor based on a NiO-Co3O4 composite material, and the preparation method thereof includes:

[0125] Step (1): add 250L of pure water to a 500L reactor until the reactor is half full, start stirring at a speed of 200r / min, heat the water to 30°C, and after the temperature in the reactor stabilizes, add 0.025kg of ammonium carbonate solid to the water in the reactor and mix well.

[0126] Step (2): After the bottom liquid environment is stable, add ammonium carbonate solution and a mixed solution formed by cobalt chloride, nickel chloride and acetic acid to the reactor in parallel, wherein the concentration of cobalt chloride in the mixed solution is 50g / L of cobalt sulfate, the concentration of nickel chloride in the mixed solution is 50g / L, the concentration of acetic acid in the mixed solution is 0.1g / L, and the flow rate of the mixed solution is 25L / h. Control the flow rate of the ammonium carbonate solution to keep the reaction pH at 6.0, start suction filtration after the kettle is full, keep the reactor liquid level near the overflow port, and stop feeding the liquid until the particle size of the nickel cobalt carbonate material grows to 1μm, and obtain nickel cobalt carbonate slurry (500L).

[0127] Step (3): centrifuge, wash and dry the nickel cobalt carbonate slurry. The washing water is 750L pure water, and the powder is dried in a blast oven at 100°C for 20h. The dried powder is calcined in a muffle furnace at a heating rate of 2°C / min, a calcination temperature of 400°C, and a holding time of 6h to obtain a honeycomb NiO-Co3O4 composite material.

[0128] Step (4): Grind and mix the prepared NiO-Co3O4 composite material with deionized water to form a viscous slurry; evenly apply the slurry on a ceramic tube with two gold electrodes and four platinum wires, and use the nickel-chromium alloy wire on the inside of the tube as a heating resistor of a side-heated heating device to obtain a working electrode; after drying the obtained working electrode in the shade overnight, place it in a muffle furnace and calcine it at 300°C for 30 minutes to obtain a gas sensor with stable performance.

[0129] Example 6

[0130] This embodiment provides a gas sensor based on a NiO-Co3O4 composite material, and the preparation method thereof includes:

[0131] Step (1): add 250L of pure water to a 500L reactor until the reactor is half full, start stirring at a speed of 500r / min, heat the water to 40°C, and after the temperature in the reactor stabilizes, add 2.5kg of sodium carbonate solid to the water in the reactor and mix well.

[0132] Step (2): After the bottom liquid environment is stable, sodium carbonate solution and a mixed solution formed by cobalt nitrate, nickel nitrate and acetic acid are added to the reactor in parallel, wherein the concentration of cobalt nitrate in the mixed solution is 80g / L of cobalt sulfate, the concentration of nickel nitrate in the mixed solution is 80g / L, the concentration of acetic acid in the mixed solution is 0.1g / L, and the flow rate of the mixed solution is 25L / h. The flow rate of the sodium carbonate solution is controlled to keep the reaction pH at 8.0, and the suction filtration is turned on after the reactor is full, and the reactor liquid level is kept near the overflow port until the particle size of the nickel cobalt carbonate material grows to 5μm and then the liquid is stopped to obtain nickel cobalt carbonate slurry (500L).

[0133] Step (3): centrifuge, wash and dry the nickel cobalt carbonate slurry. The washing water is 750L pure water, and the powder is dried in a blast oven at 120°C for 16 hours. The dried powder is calcined in a muffle furnace at a heating rate of 8°C / min, a calcination temperature of 700°C, and a holding time of 1 hour to obtain a honeycomb NiO-Co3O4 composite material.

[0134] Step (4): Grind and mix the prepared NiO-Co3O4 composite material with deionized water to form a viscous slurry; evenly apply the slurry on a ceramic tube with two gold electrodes and four platinum wires, and use the nickel-chromium alloy wire on the inside of the tube as a heating resistor of a side-heated heating device to obtain a working electrode; after drying the obtained working electrode in the shade overnight, place it in a muffle furnace and calcine it at 300°C for 30 minutes to obtain a gas sensor with stable performance.

[0135] Comparative Example 1

[0136] This comparative example provides a gas sensor based on a NiO-Co3O4 composite material, and the preparation method thereof includes:

[0137] Step (1): add 250L of pure water to a 500L reactor until the reactor is half full, start stirring at a speed of 400r / min, heat the water to 37°C, and after the temperature in the reactor stabilizes, add 2kg of ammonium bicarbonate solid to the water in the reactor and mix well.

[0138] Step (2): After the bottom liquid environment is stable, add ammonium bicarbonate solution and a mixed solution formed by cobalt sulfate and nickel sulfate to the reactor in parallel, wherein the concentration of cobalt sulfate in the mixed solution is 60 g / L of cobalt sulfate, the concentration of nickel sulfate in the mixed solution is 60 g / L, and the flow rate of the mixed solution is 25 L / h. Control the flow rate of the ammonium bicarbonate solution to maintain the reaction pH at 7.5, start suction filtration after the reactor is full, keep the reactor liquid level near the overflow port, and stop feeding the solution until the particle size of the nickel cobalt carbonate material grows to 4 μm, to obtain nickel cobalt carbonate slurry (500 L).

[0139] Step (3): centrifuge, wash and dry the nickel cobalt carbonate slurry. The washing water is 750L pure water, and the powder is dried in a blast oven at 110°C for 16 hours. The dried powder is calcined in a muffle furnace at a heating rate of 5°C / min, a calcination temperature of 600°C, and a holding time of 2 hours to obtain a honeycomb NiO-Co3O4 composite material.

[0140] Step (4): Grind and mix the prepared NiO-Co3O4 composite material with deionized water to form a viscous slurry; evenly apply the slurry on a ceramic tube with two gold electrodes and four platinum wires, and use the nickel-chromium alloy wire on the inside of the tube as a heating resistor of a side-heated heating device to obtain a working electrode; after drying the obtained working electrode in the shade overnight, place it in a muffle furnace and calcine it at 300°C for 30 minutes to obtain a gas sensor with stable performance.

[0141] That is, the difference between this comparative example and Example 1 is that no acetic acid structure directing agent is used in the coprecipitation process.

[0142] Comparative Example 2

[0143] The difference between this comparative example and Example 1 is that ammonia water is used instead of acetic acid as the structure directing agent.

[0144] Comparative Example 3

[0145] The difference between this comparative example and Example 1 is that the pH of the coprecipitation reaction is 5.5.

[0146] Comparative Example 4

[0147] The difference between this comparative example and Example 1 is that the pH of the coprecipitation reaction is 8.5.

[0148] Comparative Example 5

[0149] The difference between this comparative example and Example 1 is that the calcination temperature is 300°C.

[0150] Comparative Example 6

[0151] The difference between this comparative example and Example 1 is that the calcination temperature is 800°C.

[0152] Comparative Example 7

[0153] The difference between this comparative example and Example 1 is that the calcination time is 0.5 h.

[0154] Comparative Example 8

[0155] The difference between this comparative example and Example 1 is that the heating rate during the calcination process is 10° C. / min.

[0156] Test example

[0157] ①. Comparison of the structures of the NiO-Co3O4 composite materials obtained in Examples 1 to 4 and Comparative Examples 1 to 2 is shown in the following table. Figures 1 to 7 The specific surface area results of the NiO-Co3O4 composite materials obtained in Examples 1 to 4 and Comparative Examples 1 to 2 are shown in Table 1.

[0158] The difference between Examples 1 to 4 and Comparative Example 1 is that during the preparation process, the concentrations of the acetic acid structure directing agent are 0.1 g / L, 0.5 g / L, 1 g / L, 2 g / L and 0 g / L, respectively.

[0159] Depend on Figures 1 to 3 It can be seen that as the concentration of acetic acid increases, the morphology of the primary particles gradually changes from flake to granular, and the secondary spheres change from intercalated flakes to densely packed structures, and the specific surface area shows a trend of gradual increase (consistent with the trend in Table 1). Figure 5 It can be seen that when the acetic acid concentration is too high, the particles will be too small and difficult to grow into balls. Figure 6 It can be seen that when acetic acid is not used, the spherical particles are very loosely intercalated and have a very small specific surface area (consistent with the results in Table 1).

[0160] Depend on Figure 7 It can be seen that after changing the structure directing agent, the honeycomb NiO-Co3O4 composite material cannot be obtained, and the specific surface area of ​​the corresponding NiO-Co3O4 composite material is also small.

[0161] Depend on Figure 3 It can be seen that the NiO-Co3O4 composite material is a composite material of NiO and NiCo2O4.

[0162] Table 1 Specific surface area results

[0163] <![CDATA[Specific surface area (m 2 / g)]]> Example 1 21.3 Example 2 32.5 Example 3 46.2 Example 4 15.2 Comparative Example 1 9.8 Comparative Example 2 11.4

[0164] ②. The specific surface area of ​​the NiO-Co3O4 composite materials obtained in Examples 5 to 6 and Comparative Examples 3 to 8 was tested. The results are shown in Table 2.

[0165] Table 2 Specific surface area results

[0166]

[0167]

[0168] It can be seen from Table 1 and Table 2 that the specific surface area of ​​the NiO-Co3O4 composite material prepared in the embodiment of the present invention is larger than the specific surface area of ​​the NiO-Co3O4 composite material prepared in each comparative example.

[0169] ③. Taking Examples 1 to 3 and Comparative Example 1 as examples, the gas sensors obtained from the above Examples and Comparative Example were tested according to the following methods.

[0170] A. Sensitivity test

[0171] Test products: gas sensors prepared in Examples 1 to 3 and Comparative Example 1.

[0172] Test method: The hydrogen sulfide gas sensors prepared in Comparative Example 1 and Examples 1 to 3 of the present invention were placed at different operating temperatures for testing. After the baseline was stable, 10 ppm of hydrogen sulfide gas was introduced for testing.

[0173] Test results: Figure 8 It can be seen that the gas sensor prepared in Example 3 exhibits the highest response (about 521.5) at 80°C, and the sensitivity of the hydrogen sulfide gas sensor decreases sharply as the temperature further increases. The sensitivity of the gas sensor prepared in Comparative Example 1 increases slightly with increasing temperature, reaching 168.7 at 80°C, but is still lower than the sensitivity of the gas sensors prepared in Examples 1 to 3 at 100°C.

[0174] B. Tests on different gas concentrations

[0175] Test product: the gas sensor prepared in Example 3.

[0176] Test method: Place the test product at an operating temperature of 80°C for testing. After the baseline is stable, introduce hydrogen sulfide gas of different concentrations, open the test chamber, and the gas-sensitive test is completed when the baseline becomes stable again.

[0177] Test results: Fig. 9 It can be seen that the gas sensor prepared in Example 3 still has a rapid response and recovery speed to low concentration hydrogen sulfide at 80°C.

[0178] C. Selective testing

[0179] Test product: the gas sensor prepared in Example 3.

[0180] Test method: The gas sensor prepared in Example 3 was placed at an operating temperature of 80° C. for testing. After the baseline was stable, ammonia, ethylene glycol, methanol and acetone with a concentration of 10 ppm were introduced for detection.

[0181] Test results: Fig.10 It can be seen that compared with the response to 10 ppm hydrogen sulfide gas, the gas sensor prepared in Example 3 of the present invention has extremely low response to other gases, thereby proving that the gas sensor provided by the present invention has good selectivity for hydrogen sulfide gas.

[0182] In summary, the present invention adds a specific structure-directing agent, acetic acid, to make the prepared NiO-Co3O4 composite material have a larger specific surface area, provide more active sites for gas adsorption, and help improve the sensitivity of the NiO-Co3O4 composite material. The sensor with the above-mentioned NiO-Co3O4 composite material can respond quickly to low concentrations of hydrogen sulfide, has a fast response and recovery time, and has good selectivity and stability.

[0183] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A NiO-Co 3 O 4 Composite materials, It is characterized in that The NiO-Co 3 O 4 The composite material is honeycomb-shaped; and the NiO-Co 3 O 4 The specific surface area of ​​the composite material is not less than 20m 2 / g.

2. A NiO-Co as claimed in claim 1 3 O 4 A method for preparing a composite material, It is characterized in that The following steps are involved: A mixed solution containing a cobalt salt, a nickel salt and a structure directing agent is subjected to a coprecipitation reaction with a precipitant solution for providing carbonate ions until a nickel cobalt carbonate material having a target particle size is obtained; calcining the nickel cobalt carbonate material; Wherein, the structure directing agent is acetic acid.

3. The preparation method according to claim 2, It is characterized in that The preparation of the nickel cobalt carbonate material has at least one of the following characteristics: Feature 1: The cobalt salt includes at least one of cobalt chloride, cobalt sulfate and cobalt nitrate; Feature 2: The nickel salt includes at least one of nickel chloride, nickel sulfate and nickel nitrate; Feature 3: The precipitant includes at least one of ammonium bicarbonate, ammonium carbonate and sodium carbonate; Feature 4: The concentration of the cobalt salt in the mixed solution is 50 g / L to 80 g / L; Feature 5: The concentration of the nickel salt in the mixed solution is 50 g / L to 80 g / L; Feature 6: The concentration of the structure directing agent in the mixed solution is 0.1 g / L to 1 g / L; Feature 7: The pH of the coprecipitation reaction is 6 to 8; feature 8: The coprecipitation reaction is carried out under stirring conditions; preferably, the stirring speed is 200r / min to 500r / min; Feature 9: The target particle size of the nickel cobalt carbonate material is not less than 1 μm, preferably 1 μm to 5 μm.

4. The preparation method according to claim 2 or 3, It is characterized in that The mixed solution and the precipitant solution are simultaneously added into a reaction device having a base liquid to perform a co-precipitation reaction.

5. The preparation method according to claim 4, It is characterized in that The base liquid has at least one of the following characteristics: Feature 10: The base liquid is a solution containing carbonate ions; preferably, the base liquid is an aqueous solution of ammonium bicarbonate; preferably, in the aqueous solution of ammonium bicarbonate, 0.005 kg to 0.01 kg of ammonium bicarbonate is added per liter of water; Feature 11: The temperature of the base liquid is 30°C to 40°C.

6. The preparation method according to claim 2, It is characterized in that Calcination has at least one of the following characteristics: Feature 12: The calcination temperature is 400°C to 700°C; Feature 13: Calcination time is 1h to 6h; Feature 14: The heating rate of the calcination process is 2°C / min to 8°C / min.

7. The preparation method according to claim 6, It is characterized in that Before calcining, the method further includes washing and drying the nickel cobalt carbonate material; Preferably, the drying temperature is 100°C to 120°C; Preferably, the drying time is 16 h to 20 h.

8. A gas-sensitive material, It is characterized in that The gas-sensitive material comprises the NiO-Co 3 O 4 Composite materials.

9. A sensor, It is characterized in that The gas-sensitive material of the sensor includes the gas-sensitive material according to claim 8; Preferably, the sensor is a gas sensor; Preferably, the sensor comprises a ceramic piece, and a surface of the ceramic piece has an active layer formed by the gas-sensitive material; Preferably, the thickness of the active layer is 10 μm to 40 μm.

10. A NiO-Co as claimed in claim 1 3 O 4 Use of the composite material or the gas-sensitive material according to claim 8 or the sensor according to any one of claims 8 to 9 in detecting hydrogen sulfide gas.