Novel method for recovering nickel salt in high-acid and high-copper solution
Through the method of combining ion exchange membrane and sulfurization reaction, the problem of low recovery efficiency of nickel salt in high-acid and high-copper solution is solved, efficient nickel salt recovery and resource utilization are achieved, environmental pollution and production costs are reduced, and it is suitable for industrial applications.
Patent Information
- Application Number
- CN202410832871.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
When the existing technology recovers nickel salts from high-acid and high-copper solutions, the work efficiency is low and a lot of manpower is wasted. This results in a long extraction process of nickel products, high alkali consumption, and low direct recovery rate and recovery rate of nickel.
An ion exchange membrane is used to conduct a membrane dialysis to obtain the recovered acid and diffusion residual liquid. Then a sulfurizing agent is added to the diffusion residual liquid for sulfurization reaction, and nickel-containing raw materials are obtained through a neutralization reaction, and an alkaline solution is used for neutralization treatment. Achieve efficient recovery of nickel.
It achieves the recovery of more than 90% of nickel salts in high-acid and high-copper solutions, reduces environmental pollution, provides high-quality raw materials for nickel-containing products, reduces production costs, and simplifies the process, making it suitable for industrial applications.
Smart Images

Figure CN118724337A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of industrial wastewater pollution control, and specifically relates to a new method for recovering nickel salt in a high-acid and high-copper solution. Background Art
[0002] At present, most of the traditional methods for removing copper and arsenic by copper electrolysis at home and abroad first use concentrated copper electrolyte to obtain crude copper sulfate crystals, thereby taking away some impurities such as arsenic and nickel. However, since the high-value nickel element is also taken away, with the increase in the amount of crude copper smelting treatment, the total amount of nickel taken away increases greatly, resulting in a large waste of resources. Therefore, in the process of producing refined copper sulfate products from crude copper sulfate, it is necessary to recover nickel from wastewater containing copper, arsenic and nickel.
[0003] The existing traditional process for recovering nickel is to first perform diffusion dialysis to deacidify and dearsenify the copper sulfate mother liquor, then neutralize the primary diffusion residual liquid to remove copper and arsenic, and then deeply neutralize and extract high-copper, high-arsenic, and high-nickel slag as the raw material for extracting nickel. Since the nickel-containing material contains impurities such as copper and arsenic, the main grade of nickel is low, resulting in a long nickel product extraction process, a large amount of alkali consumption, and a complicated process, which greatly reduces the direct recovery rate and recovery rate of nickel. Therefore, we need to propose a new method for recovering nickel salts in high-acid and high-copper solutions to solve the above-mentioned problems, so that it can efficiently recover nickel from industrial wastewater. Summary of the invention
[0004] The purpose of the present invention is to provide a new method for recovering nickel salt in a high-acid and high-copper solution to solve the problem that the prior art mentioned in the above background technology not only has low work efficiency but also wastes a lot of manpower.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A new method for recovering nickel salts in a high-acid and high-copper solution comprises the following steps:
[0007] S1. Install an ion exchange membrane in the feed tank to separate the feed tank into a feed tank and a receiving tank;
[0008] S2. Pour the wastewater containing high acid and high copper into the feed tank, add a low concentration solution into the receiving tank, and perform a membrane dialysis using the concentration difference between the solution in the feed tank and the receiving tank to obtain the recovered acid and the diffused residual liquid, wherein the acidity of sulfuric acid in the diffused residual liquid is less than 70 g / L;
[0009] S3, adding a vulcanizing agent to the diffused residual liquid and heating it to perform a vulcanization reaction to obtain a vulcanization reaction solution;
[0010] S4, filtering and washing the sulfidation reaction solution, and collecting the sulfidation slag and the post-sulfidation liquid after washing;
[0011] S5, adding an alkaline solution to the sulfided liquid for neutralization reaction to obtain a neutralization reaction solution;
[0012] S6. Filter and wash the neutralization reaction solution to obtain neutralization residue and neutralization liquid. The obtained neutralization residue is the raw material containing nickel.
[0013] Preferably, in step S1, the ion exchange membrane is configured as an anion exchange membrane synthesized from polystyrene or polypropylene, the anion exchange membrane is fixed in the middle of the feed tank using a frame, the feed tank is divided into chambers of equal size, the two chambers are the feed tank and the receiving tank, the ion exchange membrane is sealed around the frame, and the surface of the ion exchange membrane is flat.
[0014] Preferably, in step S2, the low-concentration solution is set to be one of pure water, deionized water, distilled water, a low-concentration salt solution and a 5% alkaline dilute solution.
[0015] Preferably, the acid solution located in the receiving tank after the recovered acid is dialyzed through the ion exchange membrane is recovered and used as a supplementary acid for copper sulfate recrystallization, and the diffused residual liquid is the solution remaining in the liquid inlet tank after one membrane dialysis.
[0016] Preferably, in step S3, the sulfiding agent is set to one or more of sodium sulfide, sodium hydrosulfide and hydrogen sulfide, the mass ratio of the sulfiding agent to the diffusion residual liquid is 1:50-60, the reaction temperature of the diffusion residual liquid for sulfidation reaction is 20-80°C, the reaction time is 1-5h, the stirring speed is 100-600r / min, and the reaction endpoint potential is 0-200mv.
[0017] Preferably, in step S4, when filtering and washing and precipitating the sulfide reaction solution, the sulfide reaction solution is first filtered using a filtering device to obtain a solid precipitate and a filtered liquid, and then the solid precipitate is washed and precipitated using pure water to remove soluble substances on the surface of the solid precipitate to obtain pure sulfide slag, and the sulfide slag is taken as a copper-containing material and enters the smelting system for recycling and use, and the filtered liquid is washed with distilled water for multiple times to remove soluble substances in the filtered liquid to obtain a pure post-sulfide liquid.
[0018] Preferably, in step S5, the alkaline solution is set to be one or more of sodium hydroxide, calcium hydroxide and potassium hydroxide, and the amount of the alkaline solution added is such that the molar ratio of the alkali to the nickel content in the high-acid high-copper solution is 2-8:1.
[0019] Preferably, the reaction solution needs to be heated and stirred during the neutralization reaction of the vulcanized liquid, the reaction temperature is 40-80° C., the reaction time is 30-90 min, and the stirring speed is 100-600 r / min.
[0020] Preferably, in step S6, when filtering and washing the neutralization reaction solution, the following steps are included:
[0021] A1. Filter the neutralization reaction solution using a vacuum filter or a filter press to obtain solid matter and liquid matter;
[0022] A2. Wash the solid matter with distilled water, and then filter it through a vacuum filter or a filter press to obtain the filtered solid matter as neutralized residue;
[0023] A3, mixing the liquid substance with the liquid filtered in A2 to obtain a neutralized liquid, and then passing the neutralized liquid into a sewage treatment system for treatment.
[0024] Preferably, the nickel content in the high-acid high-copper solution is 16-18 g / L, and the nickel content in the neutralized solution is 0.01-0.04 g / L.
[0025] The novel method for recovering nickel salt from high-acid and high-copper solution proposed by the present invention has the following advantages compared with the prior art:
[0026] 1. The present invention first performs a membrane diffusion dialysis on high-acid and high-copper wastewater to obtain recovered acid and diffusion residual liquid, then adds a sulfiding agent to the diffusion residual liquid for sulfidation reaction and separation to obtain sulfided slag and post-sulfidation liquid, and finally adds an alkaline solution to the post-sulfidation liquid for neutralization reaction. The obtained neutralized slag is the raw material containing nickel. In this way, more than 90% of the nickel salts in the high-acid and high-copper solution can be recovered, and qualified raw materials are provided for high-quality nickel-containing products, thereby realizing efficient recovery and resource utilization of nickel;
[0027] 2. The method provided by the present invention does not generate new wastewater, reduces environmental pollution, is safe and environmentally friendly, and can simultaneously precipitate copper and arsenic in sections, which is beneficial to the reuse of wastewater;
[0028] 3. The vulcanizing agent and alkaline solution used in the present invention are cheap, the operation method is simple, and it is easy to industrialize, which has important economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a flowchart of the present invention;
[0030] Figure 2 It is a flow chart of the filtration process of the sulfidation reaction solution of the present invention;
[0031] Figure 3 It is a flowchart of the filtration process of the neutralization reaction solution of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] The present invention provides Figure 1-3 A new method for recovering nickel salt in a high-acid and high-copper solution is shown, comprising the following steps:
[0035] S1. Install an ion exchange membrane in the feed tank to separate the feed tank into a feed tank and a receiving tank;
[0036] The ion exchange membrane is set as an anion exchange membrane synthesized from polystyrene or polypropylene. The anion exchange membrane is fixed in the middle of the feed tank using a frame, and the feed tank is divided into chambers of equal size. The two chambers are the feed tank and the receiving tank. The ion exchange membrane is sealed around the frame, and the surface of the ion exchange membrane is flat. The anion exchange membrane contains active groups that can exchange with anions, such as -NH3 + 、-NR2H + etc., so that it has selective permeability, which is used to selectively transmit anions in high-acid and high-copper wastewater to reduce the acidity of high-acid and high-copper wastewater, which can reduce the amount of alkaline solution used in the subsequent steps, and the recovered acid can be reused, reducing the cost of treating high-acid and high-copper wastewater.
[0037] S2. Pour the wastewater containing high acid and high copper into the feed tank, add a low concentration solution into the receiving tank, and perform a membrane dialysis using the concentration difference between the solution in the feed tank and the receiving tank to obtain the recovered acid and the diffused residual liquid, wherein the acidity of sulfuric acid in the diffused residual liquid is less than 70 g / L;
[0038] The low-concentration solution is set to be one of pure water, deionized water, distilled water, a low-concentration salt solution and a 5% alkaline dilute solution. The low-concentration solution is used to generate a concentration difference between the solution in the feed tank and the solution in the receiving tank, and dialysis is performed using the concentration difference to complete the recovery and use of sulfuric acid.
[0039] The recovered acid is an acidic solution located in the receiving tank after ion exchange membrane dialysis. The recovered acid is recovered and used as a supplementary acid for copper sulfate recrystallization. The diffused residual liquid is the solution remaining in the liquid inlet tank after the first membrane dialysis.
[0040] S3, adding a vulcanizing agent to the diffused residual liquid and heating it to perform a vulcanization reaction to obtain a vulcanization reaction solution;
[0041] The sulfiding agent is set to be one or more of sodium sulfide, sodium hydrosulfide and hydrogen sulfide, the mass ratio of the sulfiding agent to the diffusion residual liquid is 1:50-60, the reaction temperature of the diffusion residual liquid for sulfidation reaction is 20-80°C, the reaction time is 1-5h, the stirring speed is 100-600r / min, and the reaction endpoint potential is 0-200mv.
[0042] S4, filtering and washing the sulfidation reaction solution, and collecting the sulfidation slag and the post-sulfidation liquid after washing;
[0043] When filtering and washing and precipitating the sulfide reaction solution, the sulfide reaction solution is first filtered using a filtering device to obtain a solid precipitate and a filtered liquid, and then the solid precipitate is washed and precipitated using pure water to remove soluble substances on the surface of the solid precipitate to obtain pure sulfide slag, and the sulfide slag is taken as a copper-containing material and enters a smelting system for recycling and use, and the filtered liquid is washed multiple times with distilled water to remove soluble substances in the filtered liquid to obtain a pure post-sulfide liquid.
[0044] S5, adding an alkaline solution to the sulfided liquid for neutralization reaction to obtain a neutralization reaction solution;
[0045] The alkaline solution is set to be one or more of sodium hydroxide, calcium hydroxide and potassium hydroxide, and the amount of the alkaline solution added is such that the molar ratio of the alkali to the nickel content in the high-acid high-copper solution is 2-8:1.
[0046] When the vulcanized liquid undergoes neutralization reaction, the reaction solution needs to be heated and stirred, the reaction temperature is 40-80° C., the reaction time is 30-90 min, and the stirring speed is 100-600 r / min.
[0047] S6. Filter and wash the neutralization reaction solution to obtain neutralization residue and neutralization liquid. The obtained neutralization residue is the raw material containing nickel.
[0048] When filtering and washing the neutralization reaction solution, the following steps are included:
[0049] A1. Filter the neutralization reaction solution using a vacuum filter or a filter press to obtain solid matter and liquid matter;
[0050] A2. Wash the solid matter with distilled water, and then filter it through a vacuum filter or a filter press to obtain the filtered solid matter as neutralized residue;
[0051] A3, mixing the liquid substance with the liquid filtered in A2 to obtain a neutralized liquid, and then passing the neutralized liquid into a sewage treatment system for treatment.
[0052] The nickel content in the high-acid high-copper solution is 16-18 g / L, the nickel content in the neutralized solution is 0.01-0.04 g / L, and the nickel recovery rate is greater than 90%.
[0053] The method first subjects the high-acid and high-copper wastewater to membrane diffusion dialysis to obtain recovered acid and diffusion residual liquid, then adds a sulfiding agent to the diffusion residual liquid for sulfidation reaction and then separates them to obtain sulfided slag and post-sulfidation liquid, and finally adds an alkaline solution to the post-sulfidation liquid for neutralization reaction. The obtained neutralized slag is the raw material containing nickel. In this way, more than 90% of the nickel salts in the high-acid and high-copper solution can be recovered, and qualified raw materials can be provided for high-quality nickel-containing products, thereby realizing efficient recovery and resource utilization of nickel.
[0054] Example 2
[0055] According to the method provided in Example 1, nickel recovery verification 1 is performed on a high-acid and high-copper solution, and the verification steps are as follows:
[0056] 1. Test the material composition of the high-acid high-copper solution to confirm the content of copper (Cu), arsenic (As), nickel (Ni) and sulfuric acid (H2SO4) in the high-acid high-copper solution, as shown in the following table:
[0057] Element Type Cu As Ni <![CDATA[H2SO4]]> Content (g / L) 49.63 23.18 17.27 150.6
[0058] 2. Perform a membrane dialysis on the high-acid and high-copper solution to obtain the diffusion residue and the recovered acid. The recovered acid can be used as a supplementary acid for the production of copper sulfate crystals. The components in the diffusion residue are tested. The test results are shown in the following table:
[0059] Element Type Cu As Ni <![CDATA[H2SO4]]> Content (g / L) 40.19 18.22 13.55 66.2
[0060] 3. Sodium sulfide was added to the diffusion residual liquid, the reaction temperature was 20°C, the reaction time was 5h, the stirring speed was 300r / min, the reaction end point potential was 200mv, and after filtering and washing, sulfide slag and post-sulfide liquid containing copper and arsenic were obtained. The components of the post-sulfide liquid were tested, and the test results are shown in the following table:
[0061] Element Type Cu As Ni Content (g / L) 0.018 0.98 13.18
[0062] 4. Add sodium hydroxide solution to the sulfided liquid, the molar ratio of sodium hydroxide to nickel is 2:1, the reaction temperature is 40°C, the reaction time is 90min, the stirring speed is 300r / min, and the neutralized slag and neutralized liquid are obtained after filtering and washing. The composition of the neutralized liquid is tested, and the test results are shown in the following table:
[0063] Element Type Cu As Ni Content (g / L) 0.010 0.46 0.033
[0064] The Ni content of the high-acid high-copper solution before recovery is 17.27, and the Ni content of the neutralized solution after recovery is 0.033. From the table, the nickel recovery rate in the neutralization process is 99.8%, which is greater than 90%. The neutralized slag can be exported as high-quality nickel raw materials, and the neutralized liquid enters the wastewater treatment process.
[0065] In the whole process, the diffusion dialysis step reduces the acidity and the amount of alkali used for neutralization precipitation, and the recovered acid can be reused, which reduces the production cost. The sulfidation step completely precipitates copper and arsenic, with a low nickel loss rate and a high recovery rate, which improves the product quality of nickel hydroxide slag.
[0066] Example 3
[0067] According to the method provided in Example 1, nickel recovery verification 2 is performed on a high-acid and high-copper solution, and the verification steps are as follows:
[0068] 1. Test the material composition of the high-acid high-copper solution to confirm the content of copper (Cu), arsenic (As), nickel (Ni) and sulfuric acid (H2SO4) in the high-acid high-copper solution, as shown in the following table:
[0069] Element Type Cu As Ni <![CDATA[H2SO4]]> Content (g / L) 50.22 24.31 16.95 148.9
[0070] 2. Perform a membrane dialysis on the high-acid and high-copper solution to obtain the diffusion residue and the recovered acid. The recovered acid can be used as a supplementary acid for the production of copper sulfate crystals. The components in the diffusion residue are tested. The test results are shown in the following table:
[0071] Element Type Cu As Ni <![CDATA[H2SO4]]> Content (g / L) 41.36 18.69 14.13 63.6
[0072] 3. Sodium hydrosulfide was added to the diffusion residual liquid, the reaction temperature was 50°C, the reaction time was 3h, the stirring speed was 200r / min, the reaction end point potential was 100mv, and after filtering and washing, sulfide slag and post-sulfide liquid containing copper and arsenic were obtained. The components of the post-sulfide liquid were tested, and the test results are shown in the following table:
[0073] Element Type Cu As Ni Content (g / L) 0.022 0.69 13.21
[0074] 4. Add calcium hydroxide solution to the sulfided liquid, the molar ratio of calcium hydroxide to nickel is 5:1, the reaction temperature is 60°C, the reaction time is 60min, the stirring speed is 200r / min, and the neutralized slag and neutralized liquid are obtained after filtering and washing. The composition of the neutralized liquid is tested, and the test results are shown in the following table:
[0075] Element Type Cu As Ni Content (g / L) 0.011 0.51 0.030
[0076] The Ni content of the high-acid high-copper solution before recovery is 16.95, and the Ni content of the neutralized solution after recovery is 0.030. From the table, the nickel recovery rate in the neutralization process is 99.8%, which is greater than 90%. The neutralized slag can be exported as high-quality nickel raw material, and the neutralized liquid enters the wastewater treatment process.
[0077] Example 4
[0078] According to the method provided in Example 1, nickel recovery verification three is performed on a high-acid and high-copper solution, and the verification steps are as follows:
[0079] 1. Test the material composition of the high-acid high-copper solution to confirm the content of copper (Cu), arsenic (As), nickel (Ni) and sulfuric acid (H2SO4) in the high-acid high-copper solution, as shown in the following table:
[0080] Element Type Cu As Ni <![CDATA[H2SO4]]> Content (g / L) 52.64 26.13 18.25 156.7
[0081] 2. Perform a membrane dialysis on the high-acid and high-copper solution to obtain the diffusion residue and the recovered acid. The recovered acid can be used as a supplementary acid for the production of copper sulfate crystals. The components in the diffusion residue are tested. The test results are shown in the following table:
[0082] Element Type Cu As Ni <![CDATA[H2SO4]]> Content (g / L) 42.98 18.07 15.78 59.2
[0083] 3. Add hydrogen sulfide to the diffusion residual liquid, the reaction temperature is 80°C, the reaction time is 1h, the stirring speed is 400r / min, the reaction end point potential is 0mv, and after filtering and washing, sulfide slag and post-sulfide liquid containing copper and arsenic are obtained. The composition of the post-sulfide liquid is tested, and the test results are shown in the following table:
[0084] Element Type Cu As Ni Content (g / L) 0.008 0.28 12.18
[0085] 4. Add potassium hydroxide solution to the sulfided liquid, the molar ratio of potassium hydroxide to nickel is 8:1, the reaction temperature is 80°C, the reaction time is 30min, the stirring speed is 400r / min, and the neutralized slag and neutralized liquid are obtained after filtering and washing. The composition of the neutralized liquid is tested, and the test results are shown in the following table:
[0086] Element Type Cu As Ni Content (g / L) 0.006 0.012 0.019
[0087] The Ni content of the high-acid high-copper solution before recovery is 18.25, and the Ni content of the neutralized solution after recovery is 0.019. From the table, the nickel recovery rate in the neutralization process is 99.8%, which is greater than 90%. The neutralized slag can be exported as high-quality nickel raw material, and the neutralized liquid enters the wastewater treatment process.
[0088] The method does not generate new wastewater, reduces environmental pollution, is safe and environmentally friendly, and can simultaneously precipitate copper and arsenic in sections, which is beneficial to the reuse of wastewater. The sulfiding agent and alkaline solution used are cheap, the operation method is simple, and it is easy to industrialize, thus having important economic and social benefits.
[0089] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A new method for recovering nickel salts from a high-acid, high-copper solution, characterized in that: The steps include: S1. Install an ion exchange membrane in the feed tank to separate the feed tank into a feed tank and a receiving tank; S2. Pour the wastewater containing high acid and high copper into the feed tank, add a low concentration solution into the receiving tank, and perform a membrane dialysis using the concentration difference between the solution in the feed tank and the receiving tank to obtain the recovered acid and the diffused residual liquid, wherein the acidity of sulfuric acid in the diffused residual liquid is less than 70 g / L; S3, adding a vulcanizing agent to the diffused residual liquid and heating it to perform a vulcanization reaction to obtain a vulcanization reaction solution; S4, filtering and washing the sulfidation reaction solution, and collecting the sulfidation slag and the post-sulfidation liquid after washing; S5, adding an alkaline solution to the sulfided liquid for neutralization reaction to obtain a neutralization reaction solution; S6. Filter and wash the neutralization reaction solution to obtain neutralization residue and neutralization liquid. The obtained neutralization residue is the raw material containing nickel.
2. A new method for recovering nickel salts in a high-acid, high-copper solution according to claim 1, characterized in that: In step S1, the ion exchange membrane is set as an anion exchange membrane synthesized from polystyrene or polypropylene. The anion exchange membrane is fixed in the middle of the feed liquid tank using a frame, and the feed liquid tank is divided into chambers of equal size. The two chambers are the feed tank and the receiving tank respectively. The ion exchange membrane is sealed around the frame, and the surface of the ion exchange membrane is made flat.
3. A new method for recovering nickel salts in a high-acid, high-copper solution according to claim 2, characterized in that: In step S2, the low-concentration solution is set to be one of pure water, deionized water, distilled water, a low-concentration salt solution and a 5% alkaline dilute solution.
4. A new method for recovering nickel salts in a high-acid, high-copper solution according to claim 3, characterized in that: The recovered acid is an acidic solution located in the receiving tank after ion exchange membrane dialysis. The recovered acid is recovered and used as a supplementary acid for copper sulfate recrystallization. The diffused residual liquid is the solution remaining in the liquid inlet tank after the first membrane dialysis.
5. A new method for recovering nickel salts in a high-acid, high-copper solution according to claim 4, characterized in that: In step S3, the sulfiding agent is set to one or more of sodium sulfide, sodium hydrosulfide and hydrogen sulfide, the mass ratio of the sulfiding agent to the diffusion residual liquid is 1:50-60, the reaction temperature of the diffusion residual liquid for sulfidation reaction is 20-80°C, the reaction time is 1-5h, the stirring speed is 100-600r / min, and the reaction endpoint potential is 0-200mv.
6. A new method for recovering nickel salts in a high-acid, high-copper solution according to claim 5, characterized in that: In step S4, when filtering and washing and precipitating the sulfide reaction solution, the sulfide reaction solution is first filtered using a filtering device to obtain a solid precipitate and a filtered liquid, and then the solid precipitate is washed and precipitated with pure water to remove soluble substances on the surface of the solid precipitate to obtain pure sulfide slag, and the sulfide slag is taken as a copper-containing material and enters the smelting system for recycling and use, and the filtered liquid is washed with distilled water for multiple times to remove soluble substances in the filtered liquid to obtain a pure post-sulfide liquid.
7. A new method for recovering nickel salts in a high-acid, high-copper solution according to claim 6, characterized in that: In step S5, the alkaline solution is set to be one or more of sodium hydroxide, calcium hydroxide and potassium hydroxide, and the amount of the alkaline solution added is such that the molar ratio of the alkali to the nickel content in the high-acid high-copper solution is 2-8:
1.
8. A new method for recovering nickel salts in a high-acid and high-copper solution according to claim 7, characterized in that: When the vulcanized liquid undergoes neutralization reaction, the reaction solution needs to be heated and stirred, the reaction temperature is 40-80° C., the reaction time is 30-90 min, and the stirring speed is 100-600 r / min.
9. A new method for recovering nickel salts in a high-acid and high-copper solution according to claim 8, characterized in that: In step S6, when filtering and washing the neutralization reaction solution, the following steps are included: A1. Filter the neutralization reaction solution using a vacuum filter or a filter press to obtain solid matter and liquid matter; A2. Wash the solid matter with distilled water, and then filter it through a vacuum filter or a filter press to obtain the filtered solid matter as neutralized residue; A3, mixing the liquid substance with the liquid filtered in A2 to obtain a neutralized liquid, and then passing the neutralized liquid into a sewage treatment system for treatment.
10. A new method for recovering nickel salts in a high-acid and high-copper solution according to claim 9, characterized in that: The nickel content in the high-acid high-copper solution is 16-18 g / L, and the nickel content in the neutralized solution is 0.01-0.04 g / L.
Citation Information
Patent Citations
Comprehensive treatment method of acidic etching waste liquid
CN101792220A
Method for recycling copper from acid copper chloride etching liquid
CN101899665A
Method for recycling valuable metals in peracid waste fluid produced during copper anode mud treating process
CN105441685A
Arsenic-containing sulfuric acid waste acid purifying and reusing technology
CN107311363A
Desalting aqueous streams via filled cell electrodialysis
US6017433A