Electronic component
By using a combination of cordierite or Indian stone phase and forsterite covering layer in the ceramic sintered body, the problem of low dielectric constant, high strength and high Q value of the ceramic sintered body is solved, and high performance in electronic components is achieved. Improved frequency characteristics and durability.
Patent Information
- Application Number
- CN202410341138.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-01
AI Technical Summary
Existing ceramic sintered bodies have difficulties in balancing low dielectric constant, high strength and high Q value, making it difficult to achieve at a production level.
A glass-ceramic sintered body containing main phase particles of cordierite or Indian stone phase and a covering layer of forsterite or composite oxide is used to achieve both low dielectric constant, high strength and high Q value by controlling the particle size and covering layer thickness.
It achieves the balance of low dielectric constant, high strength and high Q value in electronic components, improves the frequency characteristics and durability of the components, and is suitable for high-frequency applications.
Smart Images

Figure CN118724464A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electronic component including, for example, a glass ceramic sintered body. Background Art
[0002] In ceramics used for electronic components such as capacitors, inductors, and substrates, materials with a low dielectric constant (ε) (eg, the composition disclosed in Patent Document 1) are generally used to reduce parasitic capacitance generated between internal conductors and terminals.
[0003] In recent years, electronic components require high-frequency characteristics due to the development of the fifth-generation mobile communication system. Electronic components that require high-frequency characteristics need to have a further low dielectric constant due to concerns about noise caused by parasitic capacitance. In addition, in recent years, due to the development of electric vehicles, there is a need for low dielectric constants and improved component strength. However, in order to improve the above-mentioned characteristics, the development of the composition of the core material is underway, but when used as a ceramic sintered body, it is still difficult to balance low dielectric constants, high strength, and high Q values, and the actual situation is that it has not yet reached production.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-168557 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] In view of such actual conditions, an object of the present invention is to provide an electronic component that can achieve a low dielectric constant, high strength, and a high Q value.
[0009] Technical means for solving technical problems
[0010] In order to achieve the above-mentioned object, an electronic component according to a preferred embodiment of the present invention is an electronic component including a glass ceramic sintered body.
[0011] The glass ceramic sintered body has:
[0012] Main phase particles comprising at least one of a cordierite phase and an indialite phase; and
[0013] A covering layer includes a forsterite phase that covers the main phase particles.
[0014] In the electronic component of this embodiment, it is possible to achieve a balance between low dielectric constant, high strength, and high Q value. The reason for this is not necessarily clear, but it is speculated as follows, for example. Generally, the cordierite phase and the indigo phase, especially the indigo phase, have a relatively low thermal expansion coefficient compared to forsterite. Therefore, it is believed that by covering the main phase particles with a relatively low thermal expansion coefficient with a covering layer with a relatively high thermal expansion coefficient, stress is continuously applied to the main phase particles, and cracks are difficult to progress when stress is applied from the outside. Therefore, it is possible to achieve a balance between low dielectric constant and high strength, and it is also possible to maintain a high Q value.
[0015] Furthermore, an electronic component according to another preferred embodiment of the present invention is an electronic component including a glass ceramic sintered body.
[0016] The glass ceramic sintered body has:
[0017] main phase particles comprising a composite oxide containing Si, Mg, and Al as main components; and
[0018] The covering layer exists so as to cover the main phase particles and includes a composite oxide containing Mg, Si, and Zn as main components.
[0019] For example, a composite oxide containing Si, Mg, and Al as main components in a cordierite phase or an indigostone phase has a relatively lower thermal expansion coefficient than a composite oxide containing Mg, Si, and Zn as main components in a forsterite phase. Therefore, it is considered that by covering the main phase particles with a relatively low thermal expansion coefficient with a covering layer with a relatively high thermal expansion coefficient, stress is continuously applied to the main phase particles, and cracks are difficult to develop when stress is applied from the outside, so that both low dielectric constant and high strength can be achieved, and a high Q value can be maintained.
[0020] The main phase particles are preferably indigo stone phase. Indigo stone has a higher Q value than cordierite, so both low dielectric constant and high strength can be achieved, and the Q value is further improved.
[0021] The particle size of the main phase particles is preferably 0.35 μm or more. The larger the particle size, the higher the strength of the electronic component tends to be. However, if the particle size is too large, the Q value tends to decrease and the dielectric constant tends to increase.
[0022] The thickness of the cover layer is preferably 0.02 μm or more.
[0023] It is believed that by keeping the thickness of the covering layer (e.g., corresponding to the amount of forsterite / or corresponding to the amount of the composite oxide containing Mg, Si and Zn as main components) within an appropriate range, the stress from the covering layer to the main phase particles is kept within an appropriate range, and the generation of cracks can be suppressed. Furthermore, by keeping the thickness of the covering layer within an appropriate range, the strength of the electronic component is improved. It is believed that this can appropriately maintain the compressive stress applied to the main phase particles and improve the strength.
[0024] Preferably, the covering layer may also include a forsterite phase (or a composite oxide containing Mg, Si and Zn as main components, with Mg being more than Zn / the same below) and a willemite phase (or a composite oxide containing Mg, Si and Zn as main components, with Zn being more than Mg / the same below). By constituting a part of the covering layer with the willemite phase, the dielectric constant can be reduced and the Q value can be increased.
[0025] The area ratio of the willemite phase in the covering layer to the total area of the forsterite phase and the willemite phase is preferably 0 to 73%, 1 to 73%, or 7 to 70%. If the willemite phase is too much, the strength is reduced and the thermal expansion coefficient is reduced, which tends to be difficult to be fired simultaneously with the electrode (such as Ag).
[0026] The coating layer preferably contains Ce or Cu. By containing Ce or Cu in a part of the coating layer, the strength becomes higher. It is considered that these elements are not contained in the sintered body as filler particles, but diffused into the coating layer or the surface of the main phase particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a cross-sectional view of a chip coil which is an electronic component according to one embodiment of the present invention.
[0028] Figure 2A This is an image obtained by analyzing a part of the cross section of the glass ceramic sintered body of the example of the present invention by STEM-EDS.
[0029] Figure 2B This is an image obtained by analyzing a part of the cross section of a glass ceramic sintered body according to a comparative example of the present invention using STEM-EDS.
[0030] Figure 3A This is an image obtained by analyzing a part of the cross section of the glass-ceramic sintered body of the example of the present invention by XRD.
[0031] Figure 3B This is an image obtained by analyzing a part of the cross section of a glass ceramic sintered body according to a comparative example of the present invention by XRD.
[0032] Explanation of symbols:
[0033] 1…chip coil, 2…ceramic layer, 2a1…main phase particles (cordierite / indigofera), 2b1…covering layer (forsterite), 2c1…auxiliary covering layer (willemite), 2d1…first subphase particles (cerium oxide), 2e1…second subphase particles (silicon oxide), 2a2…main phase particles (cordierite), 2b2…main phase surface layer (zinc-rich), 2c2…third subphase particles (willemite), 2d2…fourth subphase particles (forsterite / enstatite), 2e2…amorphous phase (silicon oxide), 3…internal electrode layer, 3a, 3b…lead-out electrodes, 30…coil conductor, 4…chip body, 5…terminal electrode. DETAILED DESCRIPTION
[0034] The following describes the embodiments of the present invention. However, the present invention is not limited to the embodiments described below. In addition, the components shown below include deformations or analogs that can be easily conceived by those skilled in the art. Furthermore, the components described below can be appropriately combined.
[0035] (Coil electronic components)
[0036] like Figure 1 As shown, as an electronic component according to one embodiment of the present invention, a chip coil 1 includes a chip element 4 in which ceramic layers 2 and internal electrode layers 3 are alternately stacked along the Z-axis direction.
[0037] Each internal electrode layer 3 in each layer has a ring shape (circular, elliptical or polygonal) or C shape when viewed from the Z-axis direction, and is spirally connected by through-hole electrodes (omitted in the figure) or step electrodes that penetrate the internal electrodes of adjacent ceramic layers 2 to form a coil conductor 30.
[0038] Terminal electrodes 5 are formed at both ends of the chip element 4 in the Y-axis direction. The ends of the lead electrodes 3a and 3b that are led out to opposite sides along the Y-axis from the spirally continuous coil conductor 30 are connected to each terminal electrode 5. That is, each terminal electrode 5 is connected to both ends of the coil conductor 30 that constitutes a closed magnetic circuit coil (winding pattern).
[0039] In this embodiment, the stacking direction of the ceramic layer 2 and the internal electrode layer 3 is consistent with the Z axis, the upper and lower surfaces of the chip element 4 are parallel to the XY plane, and the end surface opposite to the Y axis forming the terminal electrode 5 is parallel to the XZ plane. In addition, the X axis, Y axis and Z axis are perpendicular to each other. Figure 1 In the illustrated multilayer chip coil 1 , the winding axis of the coil conductor 30 substantially coincides with the Z axis.
[0040] There is no particular restriction on the shape or size of the chip element 4, which can be appropriately set according to the application. Usually, the shape is roughly rectangular, for example, the X-axis size is 0.1-0.8mm, the Y-axis size is 0.2-1.6mm, and the Z-axis size is 0.1-1.0mm.
[0041] In addition, there are no special restrictions on the inter-electrode thickness and base thickness of the ceramic layer 2. The inter-electrode thickness (the interval between the internal electrode layers 3 and 3) can be set to a range of 2 to 50 μm, and the base thickness (the distance from the Z-axis end of the coil conductor 30 to the upper and lower surfaces of the chip body 4) can be set to a range of 5 to 300 μm.
[0042] In this embodiment, the terminal electrodes 5 are not particularly limited, and are formed by applying a conductive paste mainly composed of Ag or Pd to the outer surface of the element body 4, baking it, and then performing electroplating. For the electroplating, Cu, Ni, Sn, etc. can be used.
[0043] The coil conductor 30 preferably contains Ag (an alloy containing Ag), and is composed of, for example, simple Ag, an Ag-Pd alloy, etc. In addition, the coil conductor may contain Cu, Zr, Si, Al, Ti, Mg, and oxides thereof as subcomponents.
[0044] The ceramic layer 2 is composed of a glass ceramic sintered body according to one embodiment of the present invention. The glass ceramic sintered body will be described in detail below.
[0045] (Glass ceramic sintered body)
[0046] like Figure 2A As shown in the cross-sectional image of STEM-EDS, the glass ceramic sintered body of the present embodiment constituting the ceramic layer 2 has a main phase particle 2a1 as a crystal particle, and a covering layer 2b1 and an auxiliary covering layer 2c1 that exist in a manner of covering the main phase particle 2a1. In addition, "existing in a manner of covering the main phase particle 2a1" in the cross-sectional image does not need to exist in a manner of completely covering the main phase particle 2a1, and it is sufficient as long as it exists in a manner of covering more than 50% of the periphery of the main phase particle 2a1, or it may also exist in a manner of covering more than 80%.
[0047] In the present embodiment, the main phase grains 2a1 are composed of a composite oxide containing Si, Mg and Al as main components, and may contain oxides of Zn, Zr, Ce, Cu, B, Ca, Sr, Ba, Li, Na, K, etc. as other components. In addition, in the present embodiment, "elements contained as main components" refer to elements whose content ratio converted to oxides of each element contained as main components is 10 mass % (or mol % / the same below) or more.
[0048] In this embodiment, the main phase particles 2a1 are composed of a cordierite phase or an indigo phase, preferably an indigo phase. Whether the main phase particles 2a1 are composed of a cordierite phase or an indigo phase can be determined, for example, by the results of STEM-EDS (e.g. Figure 2A or Figure 2B ) and XRD analysis (e.g. Figure 3A or Figure 3B ) to find the answer.
[0049] The particle size of the main phase particles 2a1 is preferably 0.35 μm or more, 0.4 μm or more, 0.5 μm or more, or 0.55 μm or more, and preferably 2.2 μm or less, 2.15 μm or less, 2.0 μm or less, or 1.9 μm or less. The larger the particle size, the higher the strength of the chip coil 1 as an electronic component, but when the particle size is too large, the Q value tends to decrease and the dielectric constant tends to increase. In the chip coil 1 corresponding to high frequencies, it is preferred that the dielectric constant is low.
[0050] The particle size of the main phase particles 2a1 can be obtained, for example, by finding the area of each main phase particle 2a1 from a cross-sectional image of an SEM, setting the diameter of an imaginary perfect circle having the area as the particle size, and finding it as an average of 300 or more main phase particles 2a1 randomly selected. In addition, the observation magnification of the cross-sectional image of the SEM is appropriately adjusted at 2000 to 10000 times so that 300 or more main phase particles are included in one field of view.
[0051] In the present embodiment, the cover layer 2b1 is composed of a forsterite phase, but may include an auxiliary cover layer 2c1 composed of a willemite phase. It can also be said that the cover layer 2b1 is composed of a composite oxide containing Mg, Si and Zn as main components, with Mg being greater than Zn. The cover layer 2b1 may also contain oxides of Al, Zr, Ce, Cu, B, Ca, Sr, Ba, Li, Na, K, etc. as other components.
[0052] In addition, it can be said that the auxiliary covering layer 2c1 is composed of a composite oxide containing Mg, Si and Zn as main components, and Zn is more than Mg. The auxiliary covering layer 2c1 may also contain oxides of other components as the covering layer 2b1 as other components. By containing Ce or Cu in a part of the covering layer 2b1 (2c1), the strength of the electronic component is increased. It is believed that these elements are not contained in the sintered body as filler particles, but diffused into the surface of the covering layer 2b1 (2c1) or the main phase particles 2a1.
[0053] The cover layer 2 b 1 composed of the forsterite phase includes the auxiliary cover layer 2 c 1 composed of the willemite phase, so that the dielectric constant can be reduced and the Q value can be improved.
[0054] The thickness of the cover layer 2b1 (including the auxiliary cover layer 2c1 and the same below) is preferably 0.02 μm or more, 0.025 μm or more, or 0.05 μm or more, and preferably 0.6 μm or less, 0.55 μm or less, or 0.5 μm or less.
[0055] It is believed that by keeping the thickness of the covering layer 2b1 (for example, corresponding to the amount of forsterite / or corresponding to the amount of the composite oxide containing Mg, Si and Zn as main components) within an appropriate range, the thermal expansion coefficient of the covering layer 2b1 can be kept within an appropriate range, thereby suppressing the occurrence of cracks. In addition, for example, it is also easy to sinter simultaneously with the internal electrode layer (for example, Ag) 3. Furthermore, by keeping the thickness of the covering layer 2b1 within an appropriate range, the strength of the chip coil 1 is improved. It is believed that this can appropriately maintain the compressive stress applied to the main phase particles 2a1 and improve the strength.
[0056] In addition, the thickness of the cover layer 2b1 can be determined, for example, from Figure 2A In the image obtained by STEM-EDS shown in the figure, the thickness of the portion having a different contrast from the main phase grain 2a1 and extending in a manner surrounding the main phase grain 2a1 is measured at more than 50 points, and the average value thereof is taken as the thickness of the covering layer 2b1 and the auxiliary covering layer 2c1. At this time, the observation magnification is set to 5,000 to 20,000 times, and is appropriately adjusted in a manner that more than 30 main phase grains are included in one field of view. In addition, in the present embodiment, in the cross-sectional image of the ceramic sintered body within the range of 7.5μm×7.5μm, it is preferred that there are more than 30, or more than 20, main phase grains 2a1 whose surroundings are covered by more than 50% of the covering layer 2b1 and the auxiliary covering layer 2c1.
[0057] Or, for example, Figure 2A Similarly, from the element distribution of Mg measured by STEM-EDS, the thickness of the Mg layer covering the main phase grain 2a1 at more than 50 points is measured, and the average value is taken as the thickness of the covering layer 2b1. Mg is the most abundant element in the main component elements constituting the covering layer 2b1 composed of the forsterite phase. In addition, the thickness of the auxiliary covering layer 2c1 composed of the willemite phase can also be calculated by Figure 2A Similarly, from the Zn element distribution measured by STEM-EDS, the thickness of the Zn layer covering the portion of the main phase grain 2a1 at 50 or more points is measured, and the average value is taken as the thickness of the auxiliary covering layer 2c1. In addition, Zn is the most abundant element contained in the main component elements constituting the auxiliary covering layer 2c1 composed of the willemite phase.
[0058] like Figure 2AAs shown, the ceramic sintered body constituting the ceramic layer may also contain first subphase particles 2d1 and second subphase particles 2e1 as other particles. The first subphase particles 2d1 are preferably mainly composed of Ce oxide and / or Cu oxide, and exist as a part of the covering layer 2b1 or the auxiliary covering layer 2c1. The content ratio of Ce and / or Cu in the first subphase particles 2d1 is, for example, 95% by mass or more, or 97% by mass or more in terms of oxide conversion, and may contain, for example, less than 5% by mass, or less than 3% by mass of oxides of Si, Zn, Al, etc. as other components.
[0059] The second subphase particles 2e1 may be mainly composed of Si oxides and exist as a part of the covering layer 2b1 or the auxiliary covering layer 2c1. The content ratio of Si in the second subphase particles 2e1 is, for example, 95% by mass or more, or 97% by mass or more in terms of oxide conversion, and may contain, for example, less than 5% by mass, or less than 3% by mass of oxides of Mg, Zn, Al, Ce, etc. as other components. The second subphase particles 2e1 may also be contained as a filler composed of SiO2 monomer, a filler composed of Al2O3 monomer, or a filler composed of composite oxides thereof.
[0060] In the present embodiment, when 30 or more main phase grains 2a1 are included in one field of view of STEM-EDS, the area ratio of the main phase grains 2a1 in one field of view is preferably 30 to 70%, or 40 to 60%.
[0061] In addition, under the same conditions, the total area ratio of the covering layer 2b1 and the auxiliary covering layer 2c1 (one field of view is 100%) is not particularly limited, but is smaller than the area ratio of the main phase particles 2a1, and is preferably 15 to 45%, or 20 to 40%. In addition, the area ratio of the auxiliary covering layer 2c1 to the total area of the covering layer 2b1 and the auxiliary covering layer 2c1 is preferably 0 to 73%, 1 to 73%, or 7 to 70%. When the auxiliary covering layer 2c1 composed of the willemite phase is too much, the strength is reduced, and the thermal expansion coefficient is reduced, so that it tends to be difficult to be fired simultaneously with the electrode (for example, Ag).
[0062] Furthermore, under the same conditions, the area ratio of the first subphase particles 2d1 in one field of view is preferably 1% or less, or 0.5% or less, or 0.3% or less. Furthermore, under the same conditions, the area ratio of the second subphase particles 2e1 in one field of view is preferably 15% or less, or 13% or less.
[0063] (Manufacturing method)
[0064] Next, Figure 1 The manufacturing method of the chip coil 1 shown in FIG. 1 is described below. First, a Figure 1The internal electrode layer 3 shown is a conductor paste of Ag or the like. The conductor paste can be produced by a known method.
[0065] In addition to the conductor paste, a composition including Figure 1 The ceramic paste is a raw material for the glass ceramic sintered body of the ceramic layer 2 shown in FIG. The ceramic paste contains a raw material that becomes a glass ceramic sintered body having the above-mentioned composition and crystal structure after firing. The raw material for the glass ceramic sintered body is not particularly limited, and examples thereof include Figure 2A The metal elements contained in the main phase grains 2a1 and the cover layer 2b1 shown, and the metal elements contained in the auxiliary cover layer 2c1 and / or the subphase grains 2d1, 2e1 as needed, are various oxides, various compounds, or one or more glass compositions.
[0066] For example, a ceramic paste can be obtained by pulverizing one or more glass compositions as raw materials, adding other oxide powders, sintering aids, fillers, etc., and further kneading them together with a binder and a solvent.
[0067] In addition, in this embodiment, by controlling the amount of Zn contained in the glass composition, etc., the relative position of the auxiliary cover layer 2c1 can be controlled. Figure 2A The area ratio of the total area of the cover layer 2b1 and the auxiliary cover layer 2c1 is shown. For example, by increasing the amount of Zn, the area ratio of the auxiliary cover layer 2c1 can be increased.
[0068] In addition, for example, as a filler, by adding a small amount of a large specific surface area (for example, SSA of 5m 2 / g or more) of CeO2 and / or CuO, etc., can make the covering layer 2b1 or the auxiliary covering layer 2c1 contain Ce and / or Cu. In addition, part of the filler sometimes also generates subphase particles 2d1. In addition, it is believed that silicon oxide as a filler generates subphase particles 2e1, and part of it diffuses into the covering layer 2b1 or the auxiliary covering layer 2c1.
[0069] Next, for example, the ceramic paste and the conductor paste are alternately printed, and the conductor paste patterns between different layers are connected by through holes or height differences, so that a spiral conductor pattern is formed inside the laminate of the ceramic paste layers. Next, as needed, the laminate is pressed and cut into a specified size to obtain a green chip, and the green chip is fired, thereby forming a Figure 1 The chip element 4 shown (printing method).
[0070] Alternatively, a green sheet may be made from ceramic paste, internal electrode paste may be printed on the surface of the green sheet, and these may be stacked and fired to form the chip body 4 (sheet method). In any case, after the chip body 4 is formed, the terminal electrodes 5 may be formed by sintering or plating.
[0071] There is no restriction on the content of the binder and the solvent in the ceramic paste. For example, the total amount of the ceramic paste can be set to 100 mass%, the content of the binder can be set to a range of 5 to 25 mass%, and the content of the solvent can be set to a range of 30 to 80 mass%. In addition, the paste can contain a dispersant, a plasticizer, etc. in a range of 20 mass% or less as needed.
[0072] Conductor paste containing Ag or the like can also be prepared in the same manner. In addition, the firing conditions are not particularly limited, but when the internal electrode layer contains Ag or the like, the firing temperature is preferably 960°C or less, 920°C or less, or 900°C or less, and preferably 870°C or more. By controlling the maximum temperature during firing, for example, Figure 2A The thickness of the cover layer 2b1 or the auxiliary cover layer 2c1 is shown.
[0073] The firing time is not particularly limited, but is preferably about 0.5 to 10 hours. The particle size of the main phase particles 2a1 can also be controlled by the firing time. The longer the firing time, the larger the particle size. The heating rate during firing is not particularly limited. By increasing the heating rate (for example, 3 to 10 times the normal rate), the particle size can be increased. Figure 2A The particle size of the main phase particles 2a1 is shown.
[0074] In addition, by controlling the heat treatment after firing at the highest temperature during firing, the crystal structure of the main phase grains 2a1 can also be controlled. For example, after firing at the highest temperature during firing, by extending the annealing time at a temperature lower than the highest temperature, the main phase grains 2a1 composed of cordierite are easily generated. In addition, if the annealing time after firing at the highest temperature during firing is shortened, or the temperature is lowered without annealing, the main phase grains 2a1 composed of indigo are easily generated.
[0075] (Summary of Implementation Methods)
[0076] In the chip coil 1 which is an electronic component of the present embodiment, it is possible to achieve a low dielectric constant, high strength, and a high Q value. The reason for this may not be clear, but it is speculated as follows. Generally, the thermal expansion coefficients of cordierite phase and indigo phase, especially indigo phase, are relatively low compared to forsterite. Therefore, it is believed that by covering the main phase particles with a relatively low thermal expansion coefficient with a covering layer with a relatively high thermal expansion coefficient, stress is continuously applied to the main phase particles, and cracks are difficult to progress when stress is applied from the outside. Therefore, it is possible to achieve a low dielectric constant and high strength, and it is possible to maintain a high Q value.
[0077] Alternatively, a composite oxide containing Si, Mg, and Al as main components in a manner that forms a cordierite phase or an indigostone phase has a relatively lower thermal expansion coefficient than a composite oxide containing Mg, Si, and Zn as main components in a manner that forms a forsterite phase. Therefore, it is believed that by covering the main phase particles having a relatively low thermal expansion coefficient with a covering layer having a relatively high thermal expansion coefficient and applying compressive stress to the main phase particles, it is possible to achieve both a low dielectric constant and a high strength, and to maintain a high Q value.
[0078] In addition, in this embodiment, the main phase grains 2a1 are preferably indigo stone phase. Indigo stone has a higher Q value than cordierite, so both low dielectric constant and high strength can be achieved, and the Q value is further improved.
[0079] In the present embodiment, the covering layers 2b1 and 2c1 include a forsterite phase (or a composite oxide containing Mg, Si and Zn as main components, with Mg being more than Zn / the same below) and a willemite phase (or a composite oxide containing Mg, Si and Zn as main components, with Zn being more than Mg / the same below). By forming a part of the covering layer with the willemite phase, the dielectric constant can be reduced and the Q value can be improved.
[0080] In this embodiment, the covering layers 2b1 and 2c1 contain Ce or Cu. By including Ce or Cu in a part of the covering layers 2b1 and 2c1, the strength is increased. It is believed that these elements are not included in the sintered body as filler particles, but diffused to the surface of the covering layer or the main phase particles. In addition, a part of Ce or Cu included as a raw material may enter the inside of the covering layers 2b1 and 2c1 and form oxide particles ( Figure 2A The first subphase particles 2d1) are present as shown.
[0081] In addition, the present invention is not limited to the above-mentioned embodiment, and various changes can be made within the scope of the present invention.
[0082] For example, the glass ceramic sintered body of the present embodiment can also be used as an element of a coil component integrated in a semiconductor device, etc. For example, the glass ceramic sintered body of the present embodiment can be thinned and integrated on a substrate formed with a semiconductor device.
[0083] Furthermore, the glass ceramic sintered body of the present embodiment can be suitably used as an interlayer material for a high-frequency coil.
[0084] The glass ceramic sintered body of the present embodiment has a low dielectric constant and sufficient strength, and therefore can be particularly preferably used as an interlayer material constituting the internal electrode layer 3 and the ceramic layer 2 between the internal electrode layers 3 .
[0085] The ceramic sintered body of this embodiment can improve dielectric constant, strength, and sinterability in a balanced manner, and can realize a high Q value in a high frequency region as an electronic component. The ceramic sintered body is particularly suitable for use as a high frequency coil used in a frequency range of 1 GHz or more.
[0086] In addition, in the above-mentioned present embodiment, an example is shown in which the ceramic layer 2 of the chip coil 1 is formed of the same material, but it is not necessarily formed of the same material. As mentioned above, the glass ceramic sintered body of the present embodiment is particularly suitable as an interlayer material constituting the ceramic layer 2 between the internal electrode layers 3, 3, and the ceramic layer 2 not in contact with the coil conductor 30 can also be composed of other ceramic materials.
[0087] Example
[0088] Hereinafter, the present invention will be described based on more detailed examples, but the present invention is not limited to these examples.
[0089] (Sample No. 1a)
[0090] As raw materials, 83 parts by mass or more of glass powder (magnesium-silicon-aluminum glass frit) containing Mg, Al, Zn and Si and 0.5 parts by mass or less of a glass having a specific surface area (SSA) of 6.4 m were prepared so as to make 100 parts by mass of the total. 2 / g or more of cordierite powder, 2.0 parts by mass or less of cerium oxide (CeO2), 15 parts by mass or less of a silica (SiO2) filler, and 1 part by mass or less of a sintering aid containing B are mixed by a ball mill to prepare a glass ceramic paste.
[0091] The obtained glass ceramic paste is applied to a PET film by a coating machine to form a green sheet. In addition, an Ag electrode pattern is formed on the dried green sheet by screen printing. After peeling off the PET film, the sheets are overlapped and pressed in a manner that the electrode patterns on each sheet are connected in a spiral shape, and then the obtained laminate is cut to prepare a green chip.
[0092] The green chip was sintered in the following order. The temperature was raised from room temperature to 400°C and degreased. The temperature was raised to 800°C at a rate of 1000°C / hour and then raised to 900°C at a rate of 200°C / hour. Then, the green chip was sintered at 900°C in the atmosphere for 1 hour without annealing and cooled to room temperature at a rate of 200°C / hour to obtain a green chip. Figure 1 The sample of the chip element 4 shown is cut into pieces to obtain a ceramic sintered body sample constituting the ceramic layer 2. The obtained ceramic sintered body sample and the sample of the chip element are evaluated as follows.
[0093] <Cross-Section Analysis>
[0094] The cross-sectional analysis of the sintered body samples was performed by STEM-EDS. Figure 2A The image shown. It can be confirmed that the covering layer 2b1 (part of which is the auxiliary covering layer 2c1) surrounds a plurality of main phase particles 2a1. In addition, subphase particles 2d1 and 2e1 are also observed. The composition analysis of the main phase particles 2a1 shows that the main phase particles 2a1 contain 45 to 70 mass % Si in terms of oxide, 15 to 20 mass % Mg in terms of oxide, 15 to 20 mass % Al in terms of oxide, less than 4 mass % Zn in terms of oxide, less than 0.1 mass % Ce in terms of oxide, and less than 0.2 mass % Zr in terms of oxide.
[0095] In addition, the covering layer 2b1 contains 30 to 40 mass % of Si calculated as oxide, 30 to 40 mass % of Mg calculated as oxide, less than 3 mass % of Al calculated as oxide, 20 to 30 mass % of Zn calculated as oxide, 0.1 to 0.2 mass % of Ce calculated as oxide, and 0.3 to 0.7 mol of Zr calculated as oxide.
[0096] Furthermore, XRD analysis was performed on the sintered body sample including the main phase particles 2a1 and the covering layer 2b1. The results are as follows: Figure 3A As shown, peaks of indigoite (black dots) and forsterite (X) were observed. Based on the results of STEM-EDS and XRD, it is believed that the main phase particles contain an indigoite phase and the cover layer 2b1 contains a forsterite phase.
[0097] In addition, by the same analysis method, it was found that the cover layer 2c1, which had a different image contrast from the cover layer 2b1, contained 20 to 30 mass % of Si in terms of oxide, 3 to 10 mass % of Mg in terms of oxide, 1 mass % or less of Al in terms of oxide, 60 to 70 mass % of Zn in terms of oxide, 0.1 to 0.2 mass % of Ce in terms of oxide, and 0.2 mol or less of Zr in terms of oxide. In addition to other observation results, it was determined that the cover layer 2c1 contained a willemite phase.
[0098] Furthermore, by the same analysis method, it was confirmed that the subphase grains 2d1 contained 99 mass % or more of Ce in terms of oxide, and the subphase grains 2e1 contained 99 mass % or more of Si in terms of oxide. It was confirmed that Ce was also diffused into the capping layers 2b1 and 2c1.
[0099] <Size of Main Phase Particles>
[0100] The cross-section of the sintered body sample was analyzed by SEM, and the following Figure 2A The image shown. At this time, the observation magnification was set to 2,000 to 10,000 times so that 300 or more main phase particles were included in one field of view. For more than 300 main phase particles 2a1, the circle conversion diameter was calculated from the cross-sectional area, and the average value was used as the particle size of the main phase particles. The results are shown in Table 1.
[0101] <Coating Thickness>
[0102] The cross-section of the sintered body sample was analyzed by STEM-EDS, and the following Figure 2A The image shown. At this time, the observation magnification was set to 5000 to 20000 times so that 30 or more main phase particles were contained in one field of view. For the covering layer 2b1 of more than 50 main phase particles 2a1, the thickness of the covering layer 2b1 covering the main phase particles 2a1 was randomly measured, and the average value was taken as the thickness of the covering layer. The results are shown in Table 1.
[0103] <Relative dielectric constant>
[0104] The relative dielectric constant (unitless) was measured by a resonance method (JIS R 1627) using a network analyzer (PNAN5222A manufactured by Agilent Technologies Inc.). In addition, in the present embodiment, the relative dielectric constant was set to be 5.8 or less, preferably 5.7 or less, or 5.6 or less as good. In addition, it is recorded as a dielectric constant in the table. The results are shown in Table 1.
[0105] <Intensity>
[0106] For a prismatic sample of the chip body (outer diameter 20 mm × 5 mm × 2 mm), the flexural strength of the sintered body was measured by a three-point bending test (distance between supports 15 mm) using a universal material testing machine 5543 manufactured by INSTRON Corporation. In addition, in this example, 185 MPa or more, preferably 200 MPa or more was considered good. The results are shown in Table 1.
[0107] <Q value>
[0108] The Q value was measured according to the Japanese Industrial Standard "Test Method for Dielectric Properties of Fine Ceramics for Microwaves (JIS R1627 1996 Edition)". Specifically, a cylinder (pellet) made of a glass-ceramic sintered body was fabricated, and the dielectric loss factor tanδ was calculated by the two-end short-circuited dielectric resonator method. Furthermore, 1 / tanδ = Q was set. The Q value was 630 or more, preferably as large as 700 or more, 800 or more, 900 or more, 1000 or more. The results are shown in Table 1. The Q value was measured according to the Japanese Industrial Standard "Test Method for Dielectric Properties of Fine Ceramics for Microwaves (JIS R1627 1996 Edition)". Specifically, a cylinder (pellet) made of a glass-ceramic sintered body was fabricated, and the dielectric loss factor tanδ was calculated by the two-end short-circuited dielectric resonator method. Furthermore, 1 / tanδ = Q was set. The Q value was 630 or more, preferably as large as 700 or more, 800 or more, 900 or more, 1000 or more. The results are shown in Table 1.
[0109] (Sample No. 1b)
[0110] As the glass composition, a glass composition with a lower Zn content than the glass composition used in Sample No. 1a was used, and cerium oxide was not included as an additive. Otherwise, a chip body and a sintered body sample were fabricated in the same manner as in Sample No. 1a, and the same evaluation as in Sample No. 1a was performed. The results are shown in Table 1.
[0111] In the cross-section of the glass-ceramic sintered body of this Sample No. 1b, no secondary phase particles composed of Ce oxide were observed, and a covering layer 2b1 was observed, but no auxiliary covering layer 2c1 was observed.
[0112] (Sample No. 2)
[0113] Cordierite powder, cerium oxide (CeO2), and silica (SiO2) filler were not included in the raw material powder. Moreover, after sintering at 900 °C for 1 hour, it was cooled to 850 °C in 15 minutes, annealed at 850 °C in the atmosphere for 60 minutes, and then cooled to room temperature at a rate of 200 °C / hour. Otherwise, a chip body and a sintered body sample were fabricated in the same manner as in Sample No. 1b, and the same evaluation as in Sample No. 1b was performed. The results are shown in Table 1.
[0114] In addition, in the same manner as in Example 1a, the results of photographing the STEM-EDS image of the glass-ceramic sintered body are shown in Figure 2B in.
[0115] As Figure 2BAs shown in FIG. 1 , it can be confirmed that the main phase particle 2a2 is a cordierite phase, but it is confirmed that the main phase surface layer 2b2 covering the surface contains 45-50 mass % Si in terms of oxide, 15-20 mass % Mg in terms of oxide, 5-8 mass % Al in terms of oxide, and 25-30 mass % Zn in terms of oxide, and is a main phase surface layer richer in Zn than the main phase particle 2a2, and is neither forsterite nor willemite. That is, in the sample No. 2 as a comparative example, the covering layers 2b1 and 2c1 shown in the sample Nos. 1a and 1b as examples are not observed. In the table, "-" is used in the column of the covering layer thickness to indicate that it is not observed.
[0116] In the sample No. 2 as a comparative example, the third subphase particles 2c2, the fourth subphase particles 2d2, and the amorphous phase 2e2 were observed. In addition, in the example, the amorphous phase 2e2 was not observed. It was confirmed that the third subphase particles 2c2 were composed of willemite phase, and the fourth subphase particles 2d2 were composed of forsterite phase or enstatite phase.
[0117] (Sample No. 3)
[0118] After sintering at 900°C for 1 hour, cooling to 850°C in 15 minutes, annealing at 850°C in the atmosphere for 60 minutes, and then cooling to room temperature at a rate of 200°C / hour, the same chip element sample and sintered body sample were prepared as sample No. 1b, and the same evaluation as sample No. 1b was performed. The results are shown in Table 1. It was confirmed that the main phase particles were cordierite phase.
[0119] (Sample No. 4)
[0120] A sample of a chip element and a sample of a sintered body were prepared in the same manner as Sample No. 2 except that the annealing treatment was not performed, and the same evaluation as that of Sample No. 2 was performed. The results are shown in Table 1. It was confirmed that the main phase particles were cordierite phase.
[0121] (Evaluation 1)
[0122] As shown in Table 1, in the examples of sample numbers 1a, 1b, and 3 in which the cover layer of the forsterite phase was formed, it was confirmed that high strength and high Q value could be achieved compared with the comparative examples of sample numbers 2 and 4. In particular, in the example in which the main phase particles were composed of the indigo phase, it was confirmed that the Q value and strength were particularly improved compared with the example in which the main phase particles were composed of the cordierite phase.
[0123] (Sample No. 5 to 8)
[0124] By controlling the firing time and the heating time, the size of the main phase particles was adjusted to the values recorded in Table 2. In the same manner as sample No. 3, samples of the chip element and the sintered body were prepared, and the same evaluation as sample No. 3 was performed. The results are shown in Table 2. In addition, in Table 2, when the thickness of the covering layer is confirmed to be 0.02 μm or more, the covering layer is recorded as "yes". In addition, the longer the firing time, the larger the particle size tends to be, and it can be confirmed that the particle size can be increased even if the heating rate is increased.
[0125] (Sample No. 9 to 12)
[0126] By controlling the firing time and the heating time in the same manner as sample numbers 5 to 8, the size of the main phase particles was adjusted to the values recorded in Table 2. In addition, in the same manner as sample number 1b, samples of chip elements and samples of sintered bodies were prepared and evaluated in the same manner as sample number 1b. In addition, in Table 2, when the thickness of the covering layer was confirmed to be 0.02 μm or more, the covering layer was recorded as "present". The results are shown in Table 2.
[0127] (Rating 2)
[0128] As shown in Table 2, it can be confirmed that in each example with different main phase particle sizes, a covering layer is formed, and a ceramic sintered body with low dielectric constant, high strength, and high Q value can be obtained. In addition, when the main phase particle size becomes larger, it can be confirmed that there is a tendency for the dielectric constant to increase, the strength to increase, and the Q value to decrease. In particular, in the example in which the main phase particles are composed of the indigo phase, it can be confirmed that the Q value is particularly improved compared with the example in which the main phase particles are composed of the cordierite phase.
[0129] (Sample No. 13 to 16)
[0130] Compared with Sample No. 3, the thickness of the covering layer was changed by controlling the maximum temperature and holding time during firing. In the same manner as Sample No. 3, a sintered body sample was prepared and the same evaluation as Sample No. 3 was performed. The results are shown in Table 3. In addition, it was confirmed that the higher the maximum temperature during firing, the thicker the covering layer tended to be, and the longer the holding time of the maximum temperature during firing was, the thicker the covering layer was.
[0131] In addition, a crack test was performed in the following procedure. Table 3 also shows the results of the crack test.
[0132] <Crack test>
[0133] 50 samples of the chip element bodies were prepared and crack tests were performed using the test method shown below.
[0134] For the samples of chip bodies with each sample number, after welding the sample in the center of the substrate (glass epoxy substrate, size 100mm×40mm, thickness 0.08mm), a load with a deflection of 1.2mm was applied for 5 seconds from the side different from the side to which the sample was welded (the back side of the substrate), and the appearance and internal cracks of the sample after the load was applied were evaluated.
[0135] The fewer cracks observed, the better.
[0136] (Sample No. 17 to 20)
[0137] Sintered body samples were prepared in the same manner as Sample No. 1b except that the maximum temperature during sintering was controlled to change the thickness of the coating layer compared to Sample No. 1b, and the same evaluations as Sample Nos. 13 to 16 were performed. The results are shown in Table 3.
[0138] (Rating 3)
[0139] As shown in Table 3, in each embodiment in which the thickness of the covering layer is used as a variable, it can be confirmed that a ceramic sintered body with a low dielectric constant, high strength, and high Q value can be obtained. Furthermore, it is confirmed that the dielectric constant tends to increase and the Q value tends to decrease as the thickness of the covering layer becomes thicker. In addition, it can be confirmed that if the thickness of the covering layer becomes thicker, there is a tendency for the strength to increase and the internal cracks to decrease, but if the thickness of the covering layer becomes too thick, there is a tendency for the strength to decrease and the internal cracks to increase.
[0140] (Sample No. 21 to 25)
[0141] Sintered body samples were prepared in the same manner as sample No. 3, except that the amount of Zn contained in the glass composition was controlled and the sintering temperature (maximum temperature during firing) was controlled so that the existence ratio (area ratio) of the willemite phase in the cover layer was adjusted to the value described in Table 4. The same evaluation as sample Nos. 13 to 16 was performed. The results are shown in Table 4. In Table 4, when the area ratio of forsterite in the field of view was confirmed to be 3.5% or more, forsterite was recorded as "present".
[0142] (Sample No. 26-30)
[0143] The sintered body samples were prepared in the same manner as sample No. 1b, except that the amount of Zn contained in the glass composition was controlled so that the existence ratio (area ratio) of the willemite phase in the cover layer was adjusted to the value described in Table 4, and the same evaluation as sample Nos. 17 to 20 was performed. The results are shown in Table 4. In Table 4, when the area ratio of forsterite in the field of view was confirmed to be 3.5% or more, forsterite was recorded as "present".
[0144] (Rating 4)
[0145] As shown in Table 4, in each embodiment containing forsterite in the covering layer, it can be confirmed that a ceramic sintered body with low dielectric constant, high strength and high Q value is obtained. In addition, by increasing the proportion of willemite in the covering layer, it is confirmed that there is a tendency for the dielectric constant to decrease, the strength to decrease, and the Q value to increase. As the reason for the decrease in strength and the increase in cracks, it is believed that the amount of willemite increases and the thermal expansion coefficient decreases. In addition, by increasing the amount of Zn contained in the glass composition, it can be confirmed that the proportion of willemite phase in the covering layer increases. In addition, by increasing the amount of Zn contained in the glass composition, it can be confirmed that the sintering temperature is also reduced.
[0146] (Sample No. 31~37)
[0147] Except for adjusting the amount of Ce and / or Cu oxides contained in the raw material and adjusting the ratio of CeO2 and CuO in the covering layer so as to obtain the numerical value (mass %) described in Table 5, the chip element sample and the sintered body sample were prepared in the same manner as Sample No. 3, and the same evaluation as Sample No. 3 was performed. The results are shown in Table 5. In Table 5, when the area ratio of forsterite in the field of view was confirmed to be 3.5% or more, forsterite was recorded as "present".
[0148] (Sample No. 38~44)
[0149] The amount of Ce and / or Cu oxides contained in the raw material was adjusted to obtain the numerical value (mass %) recorded in Table 5, and the mass % ratio of CeO2 and CuO in the covering layer was adjusted. In the same manner as sample number 1b, a sample of a chip element and a sample of a sintered body were prepared, and the same evaluation as sample number 1b was performed. The results are shown in Table 5. In addition, in Table 5, when the area ratio of forsterite in the field of view is confirmed to be 3.5% or more, forsterite is recorded as "present".
[0150] (Rating 5)
[0151] As shown in Table 5, in each example in which the covering layer contains Ce or Cu, it can be confirmed that a ceramic sintered body with low dielectric constant, high strength and high Q value can be obtained. Furthermore, compared with Example 3 in which the covering layer does not contain Ce and Cu, it can be confirmed that higher strength and Q value can be achieved in Examples 31 to 37. In addition, compared with Example 1b in which the covering layer does not contain Ce and Cu, it can be confirmed that higher strength and Q value can be achieved in Examples 38 to 44.
[0152] [Table 1]
[0153]
[0154] [Table 2]
[0155]
[0156] [Table 3]
[0157]
[0158] [Table 4]
[0159]
[0160] [Table 5]
[0161]
Claims
1. An electronic component, wherein: The electronic component comprises a glass ceramic sintered body, The glass ceramic sintered body has: A main phase particle comprising at least one of a cordierite phase and an indigo stone phase; and A covering layer includes a forsterite phase that exists in a manner covering the main phase particles.
2. The electronic component according to claim 1, wherein The main phase particles are the indigo phase.
3. The electronic component according to claim 1 or 2, wherein: The particle size of the main phase particles is greater than 0.35 μm.
4. The electronic component according to claim 1 or 2, wherein: The thickness of the cover layer is greater than 0.02 μm.
5. The electronic component according to claim 1 or 2, wherein: The overburden layer comprises a willemite phase.
6. The electronic component according to claim 5, wherein The area ratio of the willemite phase in the covering layer to the total area of the forsterite phase and the willemite phase is 1 to 73%.
7. The electronic component according to claim 1 or 2, wherein: The cover layer contains Ce or Cu.
8. An electronic component, wherein: The electronic component comprises a glass ceramic sintered body, The glass ceramic sintered body has: main phase particles comprising a composite oxide comprising Si, Mg, and Al as main components; and The covering layer exists so as to cover the main phase particles and includes a composite oxide including Mg, Si, and Zn as main components.
Citation Information
Patent Citations
Porcelain composition for high-frequency use, porcelain for high-frequency use and method for producing porcelain for high-frequency use
JP2001240470A
Insulating ceramic paste, ceramic electronic componet, and method for producing the same
US20160014892A1