Design method of high-performance asphalt mixture with large surface structure and dense and waterproof interior

By designing a high-performance asphalt mixture with a large surface structure and a dense interior, the problems of insufficient anti-skid durability and anti-water seepage performance in the existing technology are solved, and the high-temperature anti-deformation, low-temperature anti-cracking and anti-skid properties of the asphalt pavement are achieved. Improved driving safety and service life.

CN118724504AActive Publication Date: 2024-10-01JIANGSU SOBUTE NEW MATERIALS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310323353.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing asphalt mixture design methods are difficult to achieve both anti-skid durability, anti-water seepage performance and construction stability, resulting in short service life of asphalt pavement and insufficient driving safety.

Method used

Using a high-performance asphalt mixture design method with a large surface structure and dense interior, by adjusting the proportions of coarse aggregate, fine aggregate, asphalt, additives and fibers, the skeleton tamping gap rate, mineral aggregate gap rate and oil-stone ratio are controlled to ensure High-temperature deformation resistance, low-temperature crack resistance, slip resistance and water seepage resistance of asphalt mixtures.

Benefits of technology

It improves the durability and driving safety of asphalt pavement, enhances anti-skid durability and anti-water seepage performance, reduces gradation sensitivity, and extends the service life of asphalt mixtures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724504A_ABST
    Figure CN118724504A_ABST
Patent Text Reader

Abstract

The invention discloses a design method of a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior. According to the design method, on the basis that the coarse aggregate is controlled to form a skeleton structure through an existing standard single index, the index of the mutual contact degree CCD of the coarse aggregate is introduced. Through double-index control, it is ensured that the asphalt mixture forms a stable skeleton interlocking structure, and through control over the passing rate under specific sieve pores, the probability and stability of forming the skeleton interlocking structure by the coarse aggregate are improved. And moreover, the low-temperature crack resistance is improved by adding the additive and controlling the void rate of the mineral aggregate, the grading fluctuation range is reduced and the grading sensitivity is reduced through cooperative control of multiple grading indexes, and finally the large surface structure and the dense interior are achieved. When the asphalt mixture designed according to the design method is used for the surface layer of the asphalt pavement, the asphalt mixture has more excellent high-temperature deformation resistance, low-temperature crack resistance, water damage resistance, skid resistance and water seepage resistance, and the use durability and driving safety of the asphalt pavement are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road engineering pavement material design, and in particular, relates to a design method for a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior. Background Art

[0002] Asphalt concrete pavement has the characteristics of high mechanization in construction, comfortable and safe driving, convenient maintenance, fast traffic opening and renewable, and has become the most important structural form in my country. Asphalt pavement needs to withstand the environmental effects of high temperature in summer, severe cold in winter, rain, and ultraviolet aging for a long time under the load of vehicles. Therefore, asphalt concrete is required to have good high and low temperature performance, anti-skid, anti-seepage, and anti-aging.

[0003] However, with the gradual increase in traffic volume and heavy-loaded vehicles on my country's road traffic, on the one hand, conventional asphalt concrete has been unable to withstand the coupling effects of the environment and heavy vehicle loads, and its service life is relatively low; on the other hand, the performance of asphalt concrete is very sensitive to the mix ratio and construction quality, resulting in the asphalt pavement constructed on actual roads often failing to meet the design requirements, and being prone to various defects such as insufficient initial skid resistance, severe skid resistance attenuation, rutting, squeezing, cracking, water damage, etc., which not only has a service life far from the design level, but also threatens driving safety.

[0004] The use of high-performance admixtures or high-performance asphalt can improve the high and low temperature performance of asphalt mixtures to a certain extent and alleviate the above-mentioned road disease problems, but it cannot solve the requirements of asphalt concrete on the road surface for anti-seepage and anti-skid, and requires coordinated improvement through grading design.

[0005] Asphalt mixture, which is the surface layer of asphalt pavement, needs to consider its anti-skid and anti-water seepage performance when designing. Anti-skid performance is mainly related to the surface structural depth. The greater the structural depth, the better the anti-skid performance. Due to the requirements for the anti-water seepage performance of asphalt mixture, it is usually expected that the void ratio of the mixture is small. Generally, when the void ratio of asphalt mixture is low, the surface structural depth is also small. By increasing the amount of asphalt, fine material and mineral powder, the void ratio can be reduced and the anti-water seepage performance can be improved. However, during the rolling process of asphalt mixture, too much asphalt mortar may float up and reduce the surface structural depth. It can be found that the two are contradictory in the mixture gradation design.

[0006] At present, the design method of asphalt concrete for the surface layer of asphalt pavement is consistent with that of other surface layers. Relatively more emphasis is placed on the road performance of the asphalt mixture, while there is a lack of consideration of the surface functionality of the surface layer under driving safety requirements, especially in terms of the anti-skid durability and anti-water seepage performance of the surface layer asphalt mixture. The design control still needs to be optimized; therefore, the method of designing an asphalt mixture that combines road performance, functionality and construction stability is still missing in the industry. Summary of the invention

[0007] In view of the contradiction between the anti-skid durability and anti-water seepage performance design of the asphalt pavement surface in the existing asphalt mixture design method, the present invention provides a design method for a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior. When the asphalt mixture designed according to this design method is used in the surface layer of the asphalt pavement, it has better high-temperature deformation resistance, low-temperature crack resistance, water damage resistance, anti-skid and anti-water seepage performance than the existing conventional asphalt mixture, thereby improving the durability and driving safety of the asphalt pavement.

[0008] The present invention specifically provides the following technical solutions:

[0009] A design method for a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior, wherein the asphalt mixture includes coarse aggregate, fine aggregate, asphalt, additives, fiber and mineral powder; the design method specifically includes the following steps:

[0010] S1. Taking 4.75mm sieve hole as the boundary between coarse and fine aggregates, obtain the passing rate of each grade of coarse aggregate and fine aggregate under different sieve hole sizes, and measure the corresponding density of each grade of coarse aggregate, fine aggregate, asphalt, fiber and mineral powder;

[0011] S2. According to the passing rate and density of each grade of coarse aggregate and fine aggregate under different sieve holes obtained in step S1, the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder is initially determined to obtain the synthetic mineral gradation;

[0012] S3, according to the synthetic ore gradation obtained in step S2, determine the pass rate of the synthetic ore gradation under the sieve holes of 4.75 mm and 1.18 mm respectively; if both pass rates are within the control range, proceed to step S4; if at least one pass rate is not within the control range, return to step S2 to redesign the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder;

[0013] S4, according to the density obtained in step S1 and the synthetic ore gradation obtained in step S2, determine the coarse aggregate skeleton compaction gap ratio VCA of the synthetic ore gradation DRC ;

[0014] S5, according to the pass rate of the synthetic ore gradation obtained in step S2 under a 0.075 mm sieve hole, combined with the powder-binder ratio, determine the asphalt-stone ratio;

[0015] S6, preparing an asphalt mixture according to the synthetic mineral aggregate gradation obtained in step S2 and the asphalt-rock ratio obtained in step S5, measuring the density and volume parameters of the asphalt mixture, and making a determination;

[0016] When the following three conditions are met at the same time, it is determined to be qualified and step S7 is performed. If at least one condition is not met, it is determined to be unqualified and the process returns to step S2 to redesign the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder:

[0017] ① Coarse aggregate skeleton compaction gap ratio VCA DRC VCA of the gap ratio of the coarse skeleton of asphalt mixture mix The difference is ≥ 0.2%,

[0018] ② The mutual contact degree of coarse aggregate in asphalt mixture CCD ≥ 85%,

[0019] ③ The mineral void ratio VMA of asphalt mixture is between 17.5% and 24%;

[0020] S7, performing the following road performance verification on the qualified asphalt mixture obtained in step S6;

[0021] When the following five road performances are all qualified, it is determined to be qualified; when at least one road performance is unqualified, it is determined to be unqualified, and the process returns to step S2 to redesign the blending ratios of each grade of coarse aggregate, fine aggregate and mineral powder until an asphalt mixture that meets the following road performances is obtained:

[0022] a. The structural depth is greater than 0.9mm,

[0023] b. Water permeability coefficient is less than 30mL / min,

[0024] c. Dynamic stability at 60℃ is greater than 10,000 times / mm.

[0025] d. The maximum bending strain at -10℃ is greater than 2800με.

[0026] e. Freeze-thaw splitting strength ratio is greater than 90%.

[0027] Specifically, in the above step S3, the control range refers to a pass rate of 23% to 31% under a 4.75 mm sieve hole and a pass rate of 15% to 22% under a 1.18 mm sieve hole.

[0028] Specifically, in the above step S5, the powder-to-rubber ratio is 0.8-2.8.

[0029] Specifically, in the above step S6, the mutual contact degree CCD of the coarse aggregate in the asphalt mixture is calculated using the following formula (1):

[0030] CCD=(ρ G ×ρ GCA ) / VCA DRC (1)

[0031] Among them, ρ Gis the bulk density of the asphalt mixture (derived from the density determination in step S6 above), in g / cm 3 ρ GCA is the bulk density of the coarse aggregate (derived from the density determination in step S2 above), in g / cm 3 .

[0032] Generally, the coarse aggregate skeleton compaction gap ratio VCA in the above step S4 is DRC , the asphalt mixture coarse skeleton gap ratio VCA in the above step S6 mix , and the mineral aggregate void ratio VMA of asphalt mixture can be carried out in accordance with the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011, T0705-2011).

[0033] Whether the coarse aggregate of asphalt mixture forms a skeleton structure is related to its high temperature deformation resistance and anti-sliding durability. DRC ≥VCA mix "On the basis of the single index control of the coarse aggregate forming the skeleton structure of the asphalt mixture, the index of the mutual contact degree of the coarse aggregate CCD is introduced. Through the dual index control, it is ensured that the asphalt mixture forms a stable skeleton interlocking structure, and the probability and stability of the coarse aggregate forming the skeleton interlocking structure are improved by controlling the pass rate of the 4.75mm and 1.18mm sieve holes in the range of 23% to 31% and 15% to 22% respectively. Under this premise, on the one hand, the toughness of the asphalt mortar is enhanced by additives, the aging of the toughening components during the mixing process is reduced, and the low-temperature crack resistance of the asphalt mixture is improved. On the other hand, by controlling the mineral gap rate VMA ≥ 17.5%, a larger space is provided for accommodating high-toughness asphalt mortar, which not only increases the percentage of high-toughness asphalt mortar, but also avoids the floating of the asphalt mortar under compaction, thereby realizing a large surface structure of the asphalt mixture and a dense interior. Through the coordinated control of multiple grading indicators, the grading fluctuation range of the asphalt mixture is reduced, and the grading sensitivity of the asphalt mixture is reduced.

[0034] Furthermore, in the above-mentioned asphalt mixture, the asphalt is SBS modified asphalt, and the mass percentage of SBS in the total amount of the asphalt is 2% to 6%.

[0035] Furthermore, in the above-mentioned asphalt mixture, the additive is a high-viscosity additive, which can make the asphalt after addition have the following properties: ductility ≥30cm at 5°C, elastic recovery rate ≥97%, and dynamic viscosity ≥400000Pa·s at 60°C.

[0036] Preferably, the additive is added by direct injection.

[0037] The above-mentioned high viscosity additive can be selected from the high viscosity modifier MA200 of Jiangsu Subote New Materials Co., Ltd., or other commercially available products that can achieve the above-mentioned modified performance.

[0038] Furthermore, in the above-mentioned asphalt mixture, the fibers are selected from lignin fibers and / or polyester fibers.

[0039] Furthermore, in the above-mentioned asphalt mixture, the amount of mineral powder used is 6% to 10% of the total amount of coarse aggregate, fine aggregate and mineral powder.

[0040] Compared with the prior art, the asphalt mixture designed by the design method provided by the present invention has the following advantages:

[0041] (1) The surface structure depth is large (the requirements for the structure depth in the current specifications are that the water permeability coefficient is ≤120mL / min and the structure depth is ≥0.5mm), the anti-skid performance is good, especially the anti-skid durability is good. The large surface structure depth can also reduce the formation of road water film in rainy weather to a certain extent, thereby greatly improving the driving safety of vehicles;

[0042] (2) The interior is dense. When used as a surface layer, it can effectively prevent rainwater from entering the asphalt mixture, reduce the incidence of water damage, and further prevent rainwater from entering the asphalt surface layer and destroying the interlayer bonding layer, thus avoiding damage to the pavement layers;

[0043] (3) Strong high-temperature deformation resistance, coarse aggregate forms a skeleton-embedded structure, the asphalt mortar modified by direct high-viscosity additives has a higher softening point and greater viscosity under high temperature conditions, and the asphalt mixture has excellent anti-rutting and anti-pushing properties;

[0044] (4) Good low-temperature crack resistance. The asphalt mortar modified by direct high-viscosity additives has large ductility, good toughness, and low aging degree during the production process. The larger mineral gap ratio can accommodate more high-toughness asphalt mortar, enhancing the crack resistance of asphalt mixture;

[0045] (5) Improve the gradation stability of asphalt mixture, reduce the gradation fluctuation range of asphalt mixture through the coordinated control of multiple gradation indicators, and reduce the gradation sensitivity of asphalt mixture. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a flow chart of the design method of the high-performance asphalt mixture with large surface structure and dense and waterproof inside according to the present invention. DETAILED DESCRIPTION

[0047] The design method of the high-performance asphalt mixture with large surface structure and dense and waterproof interior provided by the present invention is as follows: Figure 1 shown.

[0048] It specifically includes the following steps:

[0049] S1. Screen the coarse and fine aggregates and determine the density of each component.

[0050] The coarse and fine aggregates were sieved with a sieve hole of 4.75 mm as the boundary, and the passing rates of each grade of coarse aggregate and fine aggregate at sieve holes of different sizes were statistically analyzed. The corresponding densities of each grade of coarse aggregate, fine aggregate, asphalt, fiber and mineral powder were also measured.

[0051] S2. According to the passing rate and density, the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder is initially planned to obtain the synthetic mineral grading.

[0052] S3. According to the synthetic aggregate grading, determine the passing rate of the synthetic aggregate grading under the sieve holes of 4.75 mm and 1.18 mm respectively.

[0053] Specifically, if both pass rates are within the control range, proceed to the following step S4;

[0054] If at least one of the above passes is not within the control range, the process returns to the above step S2 to redesign the proposed blending ratio to obtain a new synthetic mineral gradation.

[0055] The above control range specifically refers to: the pass rate under the 4.75mm sieve hole is 23% to 31%, and the pass rate under the 1.18mm sieve hole is 15% to 22%.

[0056] S4. Determine VCA based on density and synthetic aggregate grading DRC .

[0057] S5. Determine the oil-stone ratio based on the passing rate of the synthetic mineral grading under the 0.075mm sieve hole and the powder-rubber ratio.

[0058] S6. Prepare asphalt mixture according to the synthetic mineral aggregate gradation and the oil-stone ratio, measure the density and volume parameters of the asphalt mixture, and make a judgment.

[0059] The judgment criteria include the following three aspects:

[0060] ① Coarse aggregate skeleton compaction gap ratio VCA DRC VCA of the gap ratio of the coarse skeleton of asphalt mixture mix The difference is ≥ 0.2%;

[0061] ② The mutual contact degree of coarse aggregate in asphalt mixture CCD ≥ 85%;

[0062] ③ The mineral aggregate void ratio VMA of asphalt mixture is between 17.5% and 24%.

[0063] Specifically, if the above three conditions are met, it is determined to be qualified and proceeds to the following step S7;

[0064] If at least one condition is not met, it is judged as unqualified, and the process returns to the above step S2 to redesign the proposed blending ratio to obtain a new synthetic mineral grading.

[0065] More specifically, in the above criteria, CCD is calculated according to the following formula:

[0066] CCD=(ρ G ×ρ GCA ) / VCA DRC (1)

[0067] Among them, ρ G is the bulk density of asphalt mixture, in g / cm 3 ρ GCA is the bulk density of the coarse aggregate in g / cm 3 .

[0068] S7. Verify the road performance of the above-mentioned asphalt mixture.

[0069] Road performance includes the following five aspects:

[0070] a. The structural depth is greater than 0.9mm;

[0071] b. Water permeability coefficient is less than 30mL / min;

[0072] c. Dynamic stability at 60℃ is greater than 10,000 times / mm;

[0073] d. The maximum bending strain at -10℃ is greater than 2800με;

[0074] e. Freeze-thaw splitting strength ratio is greater than 90%.

[0075] Specifically, if the above five road performances are all met, it is determined to be qualified, indicating that the asphalt mixture prepared in the above step S6 meets the requirements and is a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior;

[0076] If at least one road performance does not meet the requirements, it is judged as unqualified, and the process returns to the above step S2 to redesign the proposed blending ratio to obtain a new synthetic mineral aggregate gradation until an asphalt mixture that meets the above road performance is obtained.

[0077] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and the various modifications suitable for specific intended applications.

[0078] Example 1

[0079] The design method provided in this embodiment, wherein the asphalt mixture includes two grades of coarse aggregates of 10mm-13mm and 5mm-10mm, two grades of fine aggregates of 3mm-5mm and 0-3mm, SBS modified asphalt, direct-injection high-viscosity additives, lignin fiber and mineral powder.

[0080] First, the coarse and fine aggregates are sieved and the density of each component is determined.

[0081] The coarse and fine aggregates were sieved with a sieve hole of 4.75 mm as the boundary, and the passing rates of each grade of coarse aggregate and fine aggregate at sieve holes of different sizes were statistically analyzed. The corresponding densities of each grade of coarse aggregate, fine aggregate, asphalt, fiber and mineral powder were also measured.

[0082] The screening curves of coarse and fine aggregates and mineral powder are shown in Table 1 below.

[0083] Table 1 Screening curves of coarse aggregate, fine aggregate and mineral powder

[0084]

[0085] The densities of coarse aggregate, fine aggregate and mineral powder are shown in Table 2 below.

[0086] Table 2 Density of coarse and fine aggregates and mineral powder

[0087]

[0088] In this embodiment, the relative density of SBS asphalt used to prepare the asphalt mixture is 1.013 g / cm 3 , the relative density of mineral powder is 2.802g / cm 3 The relative density of lignin fiber is 0.351 g / cm 3 .

[0089] Secondly, the blending proportions of each grade of coarse aggregate, fine aggregate and mineral powder are initially planned as shown in Table 3 below.

[0090] Table 3 Proportion of coarse aggregate, fine aggregate and mineral powder

[0091]

[0092] According to the screening curves of coarse aggregate, fine aggregate and mineral powder in Table 1 and the blending ratios of coarse aggregate, fine aggregate and mineral powder in Table 3, the synthetic mineral aggregate gradation shown in Table 4 below is obtained.

[0093] Table 4 Synthetic ore gradation

[0094]

[0095] Again, according to the synthetic mineral grading obtained in Table 4, the pass rates under 4.75mm and 1.18mm sieve holes are 29.9% and 16.8% respectively. It is determined that the pass rates of the synthetic mineral grading under 4.75mm and 1.18mm sieve holes are in the range of 23% to 31% and 15% to 22% respectively. Both pass rates are within the control range, and the following steps are continued.

[0096] Step 4: Calculate VCA based on density and synthetic aggregate gradation, referring to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011, T0705-2011). DRC The result is 39.1%.

[0097] The fifth step is to calculate the passing rate of the synthetic mineral aggregate grading under the 0.075mm sieve hole, which is specifically 11.8%; combined with the powder-rubber ratio, it is initially proposed to be 2.3, and the asphalt-stone ratio is calculated and determined according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011, T0705-2011), which is 6.2%.

[0098] Among them, the SBS content of SBS modified asphalt is 4%, and the amount of SBS asphalt used is 5.6% of the mineral material.

[0099] The dosage of the high-viscosity and high-elastic additive is 0.6% of the mineral material. The properties of the modified high-viscosity and high-elastic asphalt are as follows: the elongation at 5°C is 40cm, the elastic recovery rate is 98.1%, and the dynamic viscosity at 60°C is 460,000 Pa·s.

[0100] The fiber is specifically lignin fiber, and the amount used is 0.4% of the mineral material.

[0101] Step 6: Prepare asphalt mixture according to the synthetic aggregate gradation and asphalt-to-rock ratio, measure the density and volume parameters of the asphalt mixture, and calculate VCA according to the "Test Procedure for Asphalt and Asphalt Mixture for Highway Engineering" (JTG E20-2011, T0705-2011) mix and VMA, and calculate CCD according to the above formula (1); and make a judgment, the results are shown in Table 5 below.

[0102] Table 5 Asphalt mixture volume parameter results

[0103]

[0104] If all three conditions above are met, the system is considered qualified and the following steps are continued.

[0105] Finally, referring to the corresponding experimental methods in the Test Code for Asphalt and Asphalt Mixtures in Highway Engineering (JTG E20-2011, T0705-2011), the road performance of the above asphalt mixture was verified, and the results are shown in Table 6.

[0106] Table 6 Asphalt mixture test methods and road performance

[0107]

[0108] The above five road performances are all met and judged to be qualified, indicating that the asphalt mixture formulated and prepared in the above steps meets the requirements and is a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior.

[0109] Example 2

[0110] The design method provided in this embodiment, wherein the asphalt mixture includes three grades of coarse aggregates of 11mm-16mm, 6mm-11mm and 4mm-6mm, two grades of fine aggregates of 0-4mm, SBS modified asphalt, direct-injection high-viscosity additives, lignin fiber and mineral powder, wherein the 4th grade of aggregate is hot material screened by the hot material screen of the mixing station.

[0111] First, the coarse and fine aggregates are sieved and the density of each component is determined.

[0112] The coarse and fine aggregates were sieved with a sieve hole of 4.75 mm as the boundary, and the passing rates of each grade of coarse aggregate and fine aggregate at sieve holes of different sizes were statistically analyzed. The corresponding densities of each grade of coarse aggregate, fine aggregate, asphalt, fiber and mineral powder were also measured.

[0113] The screening curves of coarse aggregate, fine aggregate and mineral powder are shown in Table 7 below.

[0114] Table 7 Screening curves of coarse aggregate, fine aggregate and mineral powder

[0115]

[0116] The densities of coarse aggregate, fine aggregate and mineral powder are shown in Table 8 below.

[0117] Table 8 Density of coarse and fine aggregates and mineral powder

[0118]

[0119] In this embodiment, the relative density of SBS asphalt used to prepare the asphalt mixture is 1.013 g / cm 3 The relative density of the mineral powder is 2.802g / cm 3 The relative density of lignin fiber is 0.351 g / cm 3 .

[0120] Secondly, the blending proportions of each grade of coarse aggregate, fine aggregate and mineral powder are initially planned as shown in Table 9 below.

[0121] Table 9 Proportion of coarse aggregate, fine aggregate and mineral powder

[0122]

[0123] According to the screening curves of coarse aggregate, fine aggregate and mineral powder in Table 7 and the blending ratios of coarse aggregate, fine aggregate and mineral powder in Table 9, the synthetic mineral aggregate gradation shown in Table 10 below is obtained.

[0124] Table 10 Synthetic ore gradation

[0125]

[0126] Again, according to the synthetic mineral grading obtained in Table 10, the pass rates under 4.75mm and 1.18mm sieve holes are 23.6% and 13.1% respectively. It is determined whether the pass rates of the synthetic mineral grading under 4.75mm and 1.18mm sieve holes are within the range of 23% to 31% and 15% to 22% respectively.

[0127] Among them, the pass rate under the 1.18mm sieve hole is not within the control range, and the synthetic gradation is judged to be unqualified. Return to the second step above to re-formulate the blending ratio of coarse aggregate, fine aggregate and mineral powder, as shown in Table 11 below.

[0128] Table 11 Proportion of coarse aggregate, fine aggregate and mineral powder

[0129]

[0130] According to the screening curves of coarse aggregate, fine aggregate and mineral powder in Table 7 and the re-proposed blending ratios of coarse aggregate, fine aggregate and mineral powder in Table 11, the synthetic mineral aggregate gradation shown in Table 12 below is obtained.

[0131] Table 12 Synthetic ore gradation

[0132]

[0133] According to the synthetic mineral grading obtained in Table 12, the pass rates at 4.75mm and 1.18mm sieve holes are 26.4% and 16.4% respectively. It is determined that the pass rates of the synthetic mineral grading at 4.75mm and 1.18mm sieve holes are in the range of 23% to 31% and 15% to 22% respectively. Both pass rates are within the control range, so proceed with the following steps.

[0134] Step 4: Calculate VCA based on the density and synthetic aggregate gradation that meets the pass rate, referring to the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011, T0705-2011) DRCThe result is 38.4%.

[0135] According to the passing rate of synthetic mineral aggregate grading under the 0.075mm sieve hole, it is specifically 10.5%; combined with the powder-rubber ratio, it is initially proposed to be 2, and the asphalt-stone ratio is calculated and determined according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011, T0705-2011), which is 6.3%.

[0136] Among them, the SBS content of SBS modified asphalt is 4%, and the amount of SBS asphalt is 5.7% of the mineral material.

[0137] The dosage of the high-viscosity and high-elastic additive is 0.6% of the mineral material. The performance of the modified high-viscosity and high-elastic asphalt is as follows: the elongation at 5°C is 43cm, the elastic recovery rate is 97.2%, and the dynamic viscosity at 60°C is 430,000 Pa·s.

[0138] The fiber is lignin fiber, and the amount used is 0.4% of the mineral material.

[0139] Step 5: Prepare asphalt mixture according to the synthetic aggregate grading and asphalt-to-rock ratio that meets the passing rate, measure the density and volume parameters of the asphalt mixture, and calculate VCA according to the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011, T0705-2011). mix and VMA, and calculate CCD according to the above formula (1); and make a judgment, the results are shown in Table 13 below.

[0140] Table 13 Asphalt mixture volume parameter results

[0141]

[0142] The coarse skeleton gap ratio VCA of asphalt mixture under the above three conditions mix If the mineral void ratio VMA of the asphalt mixture is not met, it is judged as unqualified, and the amount of 4mm to 6mm aggregate is increased and the synthetic grading is re-drafted, as shown in Table 14 below.

[0143] Table 14 Proportion of coarse aggregate, fine aggregate and mineral powder

[0144]

[0145] According to the screening curves of coarse aggregate, fine aggregate and mineral powder in Table 9 and the blending ratios of coarse aggregate, fine aggregate and mineral powder in Table 14, the synthetic mineral aggregate gradation shown in the following Table 15 is obtained.

[0146] Table 15 Synthetic ore gradation

[0147]

[0148] According to the synthetic mineral grading obtained in Table 15, the pass rates at 4.75mm and 1.18mm sieve holes are 27.7% and 15.1% respectively. It is determined that the pass rates of the synthetic mineral grading at 4.75mm and 1.18mm sieve holes are in the range of 23% to 31% and 15% to 22% respectively. Both pass rates are within the control range, so proceed with the following steps.

[0149] According to the density and gradation of synthetic aggregate, VCA DRC The result is 41.2%.

[0150] According to the latest synthetic mineral aggregate grading, the passing rate under the 0.075mm sieve hole is specifically 10.7%; combined with the powder-rubber ratio, it is initially proposed to be 2, and the asphalt-stone ratio is calculated and determined according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011, T0705-2011), which is 6.3%.

[0151] Among them, the SBS content of SBS modified asphalt is 4%, and the amount of SBS asphalt is 5.7% of the mineral material.

[0152] The dosage of high-viscosity and high-elastic additive is 0.6% of the mineral material. The performance of the modified high-viscosity and high-elastic asphalt is as follows: the elongation at 5°C is 42cm, the elastic recovery rate is 97.7%, and the dynamic viscosity at 60°C is 410000Pa·s.

[0153] The fiber is lignin fiber, and the amount used is 0.4% of the mineral material.

[0154] According to the synthetic mineral aggregate grading and the oil-stone ratio, an asphalt mixture was prepared, and the density and volume parameters of the asphalt mixture were measured and judged. The results are shown in Table 16 below.

[0155] Table 16 Asphalt mixture volume parameter results

[0156]

[0157] If all three conditions above are met, the system is considered qualified and the following steps are continued.

[0158] Finally, referring to the corresponding experimental methods in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011, T0705-2011), the road performance of the above asphalt mixture was verified, and the results are shown in Table 17.

[0159] Table 17 Asphalt mixture test methods and road performance

[0160]

[0161] The above five road performances all meet the requirements and are judged to be qualified, indicating that the asphalt mixture prepared in the above steps meets the requirements and is a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior.

Claims

1. A design method for a high-performance asphalt mixture with a large surface structure and a dense and waterproof interior, characterized in that: Includes steps: S1. Taking 4.75mm sieve hole as the boundary between coarse and fine aggregates, obtain the passing rate of each grade of coarse aggregate and fine aggregate under different sieve hole sizes, and measure the corresponding density of each grade of coarse aggregate, fine aggregate, asphalt, fiber and mineral powder; S2. According to the passing rate and density of each grade of coarse aggregate and fine aggregate under different sieve holes obtained in step S1, the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder is initially determined to obtain the synthetic mineral gradation; S3, according to the synthetic ore gradation obtained in step S2, determine the pass rate of the synthetic ore gradation under the sieve holes of 4.75 mm and 1.18 mm respectively; if both pass rates are within the control range, proceed to step S4; if at least one pass rate is not within the control range, return to step S2 to redesign the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder; The control range refers to the pass rate of 23% to 31% under the 4.75mm sieve hole and the pass rate of 15% to 22% under the 1.18mm sieve hole. S4, according to the density obtained in step S1 and the synthetic ore gradation obtained in step S2, determine the coarse aggregate skeleton compaction gap ratio VCA of the synthetic ore gradation DRC ; S5, according to the passing rate of the synthetic ore gradation obtained in step S2 under the 0.075mm sieve hole, combined with the powder-binder ratio, determine the oil-stone ratio; wherein the powder-binder ratio is 0.8-2.8; S6, preparing an asphalt mixture according to the synthetic mineral aggregate gradation obtained in step S2 and the asphalt-rock ratio obtained in step S5, measuring the density and volume parameters of the asphalt mixture, and making a determination; When the following three conditions are met at the same time, it is determined to be qualified and step S7 is performed. If at least one condition is not met, it is determined to be unqualified and the process returns to step S2 to redesign the blending ratio of each grade of coarse aggregate, fine aggregate and mineral powder: ① Coarse aggregate skeleton compaction gap ratio VCA DRC VCA of the gap ratio of the coarse skeleton of asphalt mixture mix The difference is ≥ 0.2%, ② The mutual contact degree of coarse aggregate in asphalt mixture CCD ≥ 85%, The CCD is calculated using the following formula (1): CCD=(ρ G ×ρ GCA ) / VCA DRC (1) In formula (1), ρ G is the bulk density of asphalt mixture, in g / cm 3 ρ GCA is the bulk density of the coarse aggregate in g / cm 3 ; ③ The mineral void ratio VMA of asphalt mixture is between 17.5% and 24%; S7, performing the following road performance verification on the qualified asphalt mixture obtained in step S6; When the following five road performances are all qualified, it is determined to be qualified; when at least one road performance is unqualified, it is determined to be unqualified, and the process returns to step S2 to redesign the blending ratios of each grade of coarse aggregate, fine aggregate and mineral powder until an asphalt mixture that meets the following road performances is obtained: a. The structural depth is greater than 0.9mm, b. Water permeability coefficient is less than 30mL / min, c. Dynamic stability at 60℃ is greater than 10,000 times / mm. d. The maximum bending strain at -10℃ is greater than 2800με. e. Freeze-thaw splitting strength ratio is greater than 90%.

2. The design method according to claim 1, characterized in that: In the asphalt mixture, the asphalt is SBS modified asphalt, and the mass percentage of SBS in the total amount of the asphalt is 2% to 6%.

3. The design method according to claim 1, characterized in that: In the asphalt mixture, the additive is a high-viscosity additive, which can make the asphalt after addition have the following properties: 5°C elongation ≥30cm, elastic recovery rate ≥97%, 60°C dynamic viscosity ≥400000Pa·s.

4. The design method according to claim 3, characterized in that: The additive is added in a direct injection manner.

5. The design method according to claim 3, characterized in that: The additive is the high viscosity modifier MA200 produced by Jiangsu Subote New Materials Co., Ltd.

6. The design method according to claim 1, characterized in that: In the asphalt mixture, the fibers are selected from lignin fibers and / or polyester fibers.

7. The design method according to claim 1, characterized in that: In the asphalt mixture, the amount of the mineral powder is 6% to 10% of the total amount of the coarse aggregate, fine aggregate and mineral powder.

Citation Information

Patent Citations

  • Design method of a high-toughness ultrathin asphalt wearing layer mixture

    CN109657421A

  • Mix proportion design method of ultrathin wearing layer asphalt mixture

    CN110904764A

  • Methods for gradating and inspecting coarse aggregate for asphalt concrete

    CN1583387A

  • Mixing type semiflexible paving material and semiflexible paving structure

    JP2000302516A