Fireproof insulation board and preparation method and application thereof

By using materials such as Portland cement, fly ash and modified porous microspheres to prepare fireproof insulation boards, the problem of existing building exterior wall insulation materials supporting combustion in fires has been solved, and efficient fire prevention and insulation performance improvements have been achieved.

CN118724529AInactive Publication Date: 2024-10-01CHANGSHA SHENYU BUILDING MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410791991.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing building exterior wall insulation materials can easily become combustion accelerants when a fire occurs, causing the fire to intensify and have insufficient fire protection performance, threatening the safety of life and property.

Method used

Fireproof insulation boards are prepared using materials such as Portland cement, fly ash, modified porous microspheres and silane coupling agents. The modified porous microspheres form a porous structure through a combination of epoxy resin and phosphate to increase hardness and high temperature resistance. performance, and reduce interfacial energy and water molecule penetration through silane coupling agents.

Benefits of technology

It significantly improves the fire resistance and weather resistance of fire-resistant insulation boards, reduces heat conduction, enhances thermal insulation performance and mechanical strength, reduces water absorption and porosity, and improves the overall performance of building wall panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004900368810000091
    Figure BDA0004900368810000091
Patent Text Reader

Abstract

The invention discloses a fireproof insulation board and a preparation method and application thereof. The fireproof insulation board is prepared from the following raw materials: Portland cement, fly ash, a silane coupling agent and modified porous microspheres, the modified porous microspheres are prepared from epoxy resin, phosphate and carbamate, heat conduction can be effectively reduced by adding the modified porous microspheres, and the heat preservation performance of the fireproof heat preservation board is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal insulation materials, and in particular relates to a fireproof thermal insulation board and a preparation method and application thereof. Background Art

[0002] Building exterior wall insulation systems are increasingly becoming an important part of residential projects. The construction industry has higher and higher requirements for insulation boards. There are many types of building exterior wall insulation materials on the market, but the problem of insufficient fire resistance always exists. Once a fire occurs in a building, the insulation material will become a combustion aid, and the fire will intensify, causing huge economic losses and seriously threatening the lives and property of residents.

[0003] Therefore, it is necessary to provide a fireproof insulation board. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a fireproof insulation board which improves the fireproof performance of the insulation board.

[0005] The present invention also provides a method for preparing the fireproof heat-insulating board.

[0006] The present invention also proposes the application of the fireproof and heat-insulating board in building wall panels.

[0007] According to one aspect of the present invention, a fireproof thermal insulation board is provided, wherein the raw materials for preparing the board include: silicate cement, fly ash, silane coupling agent and modified porous microspheres;

[0008] The raw materials for preparing the modified porous microspheres include epoxy resin, phosphate and carbamate.

[0009] The embodiments according to the first aspect of the present invention have at least the following beneficial effects:

[0010] In the modified porous microspheres, epoxy resin is the main component of the basic structure, and carbamate decomposes and releases gas under heating conditions. These gases produce tiny bubbles in the mixture, and expand under the action of heat, prompting the raw material mixture to solidify and form porous microspheres. At the same time, due to the action of phosphate, a shell structure is formed on the outer layer of the porous microspheres. It can not only increase the hardness of the modified porous microsphere particles and improve the high temperature resistance, but also block water from entering the modified porous microspheres, thereby effectively reducing the open porosity and water absorption of the modified porous microspheres. Therefore, it can effectively reduce heat conduction and improve the thermal insulation performance of the fireproof insulation board; the silane coupling agent can effectively reduce the interfacial energy between the modified porous microspheres and the matrix material, reduce the penetration of harmful substances such as water molecules and oxygen, thereby improving the weather resistance and durability of the fireproof insulation board.

[0011] In some embodiments of the present invention, the fireproof insulation board comprises the following raw materials in parts by weight: 140-180 parts of silicate cement, 40-90 parts of fly ash, 25-30 parts of modified porous microspheres, and 4-6 parts of silane coupling agent.

[0012] In some embodiments of the present invention, the raw materials for preparing the fireproof thermal insulation board further include: a water reducing agent and water.

[0013] In some embodiments of the present invention, the silane coupling agent includes at least one of 3-aminopropyltrimethoxysilane, 3-(methoxy)propyltriethoxysilane and dimethoxymethylethyldioxysilane.

[0014] In some embodiments of the present invention, the silane coupling agent includes 3-aminopropyltrimethoxysilane.

[0015] 3-Aminopropyltrimethoxysilane undergoes a hydrolysis reaction in the modified porous microspheres, in which three methoxy groups react with water to generate three methanol molecules and three hydroxyl groups. After hydrolysis, the amino and hydroxyl parts in the amino silicone oil can form chemical bonds or hydrogen bonds with functional groups such as silicon or hydroxyl groups in the base material of the fireproof insulation board, thereby forming adhesion between the surfaces, improving the compatibility between the modified porous microspheres and other preparation raw materials of the fireproof insulation board, and greatly improving the mechanical strength of the insulation board.

[0016] In some embodiments of the present invention, the water reducer includes at least one of a polycarboxylic acid water reducer and an aliphatic water reducer.

[0017] In some embodiments of the present invention, the fireproof insulation board comprises the following raw materials in parts by weight: 140-180 parts of silicate cement, 40-90 parts of fly ash, 25-30 parts of modified porous microspheres, 4-6 parts of silane coupling agent, 1-2 parts of water reducer and 110-130 parts of water.

[0018] In some embodiments of the present invention, the modified porous microspheres include the following raw materials in parts by weight: 500-800 parts of epoxy resin, 300-600 parts of phosphate and 10-16 parts of carbamate.

[0019] According to a second aspect of the present invention, a method for preparing a fireproof insulation board is provided, comprising the following steps:

[0020] S1: mixing the silane coupling agent and the modified porous microspheres, and then adding the silicate, cement and fly ash to obtain a mixture;

[0021] S2: Place the mixture in the formwork, and after pouring, demoulding and curing, a fireproof insulation board is obtained.

[0022] In some embodiments of the present invention, the curing time is 8 to 11 days.

[0023] In some embodiments of the present invention, the demoulding step includes demoulding 5-6 hours after the pouring is completed.

[0024] In some embodiments of the present invention, the method for preparing the modified porous microspheres comprises:

[0025] A1. Mixing epoxy resin, curing agent and urethane to obtain a mixed solution;

[0026] A2. dropping the mixture in step A1 into the phosphate solution, stirring and solidifying to obtain particles;

[0027] A3. Separate and heat the particles.

[0028] In step A2, the carbamate-epoxy resin mixture is allowed to form fine droplets suspended in the phosphate solution to ensure that the mixture forms small particles in the phosphate solution. During this process, the epoxy resin is cured, and the carbamate decomposes to produce gas to form a porous structure. At the same time, phosphate will gradually deposit on the surface of the epoxy resin particles to form a shell. In step A3, the phosphate forms a stable phosphate coating under heating conditions.

[0029] In some embodiments of the present invention, the epoxy resin comprises bisphenol A epoxy resin.

[0030] In some embodiments of the present invention, the carbamate includes at least one of diisocyanate carbonate, azodicarbonamide and N,N'-dimethylcarbamide.

[0031] In some embodiments of the present invention, the bisphenol A epoxy resin includes at least one of E-55, E-51, E-44 and E-42.

[0032] In some embodiments of the invention, the phosphate comprises tricalcium phosphate.

[0033] In some embodiments of the present invention, the curing agent includes at least one of hexamethylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine.

[0034] In some embodiments of the present invention, in step A2, the curing temperature is 80-100°C.

[0035] In some embodiments of the present invention, in step A3, the heating temperature is 200-700°C.

[0036] According to a third aspect of the present invention, application of a fireproof and heat-insulating board in a building wall panel is proposed.

[0037] In some embodiments of the present invention, the building wall panel comprises a building exterior wall thermal insulation and fireproofing layer or a building interior partition panel. DETAILED DESCRIPTION

[0038] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0039] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0041] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0042] Example 1

[0043] This embodiment provides a fireproof insulation board and a preparation method thereof, specifically:

[0044] A method for preparing a fireproof insulation board comprises the following steps:

[0045] S1: By weight, 6 parts of 3-aminopropyltrimethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of Portland cement and 60 parts of fly ash were added and stirred at 60° C. for 3 h to obtain a mixture;

[0046] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0047] The preparation method of modified porous microspheres is:

[0048] A1. 100 parts of bisphenol A epoxy resin (E-42), 12 parts of hexamethylenediamine and 10 parts of azodicarbonamide were mixed to obtain a mixed solution 1;

[0049] A2. Prepare 300 parts of a phosphate solution having a concentration of 0.1 M, heat to 80 ° C, dropwise add the mixture 1 in step A1 into the phosphate solution, and stir at 500 rpm for 4 h to obtain particles;

[0050] A3. The particles were separated and precipitated using a centrifuge. The particles were washed with deionized water and heated at 700°C for 1 h.

[0051] Example 2

[0052] This embodiment provides a fireproof insulation board and a preparation method thereof, specifically:

[0053] A method for preparing a fireproof insulation board comprises the following steps:

[0054] S1: By weight, 6 parts of 3-aminopropyltrimethoxysilane and 30 parts of modified porous microspheres were mixed, and then 180 parts of Portland cement and 80 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0055] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0056] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0057] Example 3

[0058] This embodiment provides a fireproof insulation board and a preparation method thereof, specifically:

[0059] A method for preparing a fireproof insulation board comprises the following steps:

[0060] S1: By weight, 4 parts of 3-aminopropyltrimethoxysilane and 25 parts of modified porous microspheres were mixed, and then 150 parts of Portland cement and 80 parts of fly ash were added and stirred at 60° C. for 3 h to obtain a mixture;

[0061] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0062] The preparation method of modified porous microspheres is:

[0063] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0064] Cement and fly ash to obtain a mixture: 140 parts of Portland cement, 40 parts of fly ash, 0.25 parts of sodium carboxymethyl cellulose, 25 parts of glass fiber, 3 parts of bentonite, 8 parts of quartz sand, 2 parts of polyacrylamide, 2 parts of waste gypsum, 4 parts of tetramethylguanidinopropyltrimethoxysilane, 0.5 parts of ST 02A polycarboxylic acid high-performance water reducer, 8 parts of hydrogen peroxide, 3.5 parts of antimony trioxide, and 80 parts of water are weighed and set aside;

[0065] S2: Place the mixture in the formwork, and after pouring, demoulding and curing, a fireproof insulation board is obtained.

[0066] Example 4

[0067] This embodiment provides a fireproof insulation board and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the 3-aminopropyltrimethoxysilane in embodiment 1 is replaced by dimethoxymethylethyldioxysilane, specifically:

[0068] A method for preparing a fireproof insulation board comprises the following steps:

[0069] S1: By weight, 6 parts of dimethoxymethylethyldioxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0070] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0071] The preparation method of modified porous microspheres is:

[0072] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0073] Example 5

[0074] This embodiment provides a fireproof insulation board and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the 3-aminopropyltrimethoxysilane in embodiment 1 is replaced by 3-(methoxy)propyltriethoxysilane, specifically:

[0075] A method for preparing a fireproof insulation board comprises the following steps:

[0076] S1: By weight, 6 parts of 3-(methoxy)propyltriethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 h to obtain a mixture;

[0077] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0078] The preparation method of modified porous microspheres is:

[0079] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0080] Example 6

[0081] This embodiment provides a fireproof insulation board and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the 3-aminopropyltrimethoxysilane in embodiment 1 is replaced by 3-aminopropyltriethoxysilane, specifically:

[0082] A method for preparing a fireproof insulation board comprises the following steps:

[0083] S1: By weight, 6 parts of 3-aminopropyltriethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0084] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0085] The preparation method of modified porous microspheres is:

[0086] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0087] Comparative Example 1

[0088] This comparative example provides a method for preparing a fireproof insulation board. The difference between this comparative example and Example 1 is that the silane coupling agent is replaced with trimethoxysilane, and the other conditions are the same, specifically:

[0089] A method for preparing a fireproof insulation board comprises the following steps:

[0090] S1: By weight, 6 parts of trimethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0091] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0092] The preparation method of modified porous microspheres is:

[0093] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0094] Comparative Example 2

[0095] This comparative example provides a method for preparing a fireproof insulation board. The difference between this comparative example and Example 1 is that carbamate is replaced by sodium bicarbonate, and the other conditions are the same, specifically:

[0096] A method for preparing a fireproof insulation board comprises the following steps:

[0097] S1: By weight, 6 parts of trimethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0098] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0099] The preparation method of modified porous microspheres is:

[0100] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0101] Comparative Example 3

[0102] This comparative example provides a method for preparing a fireproof insulation board. The difference between this comparative example and Example 1 is that phosphate is replaced by sodium phosphite, and the other conditions are the same, specifically:

[0103] A method for preparing a fireproof insulation board comprises the following steps:

[0104] S1: By weight, 6 parts of trimethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0105] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0106] The preparation method of modified porous microspheres is:

[0107] The preparation method of the modified porous microspheres is the same as that in Example 1.

[0108] Comparative Example 4

[0109] This comparative example provides a method for preparing a fireproof insulation board. The difference between this comparative example and Example 1 is that the epoxy resin is replaced by magnesium silicate, and the other conditions are the same, specifically:

[0110] A method for preparing a fireproof insulation board comprises the following steps:

[0111] S1: By weight, 6 parts of trimethoxysilane and 30 parts of modified porous microspheres were mixed, and then 140 parts of silicate cement and 60 parts of fly ash were added and stirred at 60° C. for 3 hours to obtain a mixture;

[0112] S2: Place the mixture in the formwork, demould it 5 hours after pouring, and cure it for 10 days to obtain the fireproof insulation board.

[0113] The preparation method of modified porous microspheres is:

[0114] In parts by weight, 10 parts of sodium phosphite, 500 parts of magnesium silicate and 300 parts of phosphate were added into a reaction container and reacted at 500° C. for 1 hour.

[0115] Test Case

[0116] This test example tests the thermal conductivity and compressive strength of the fireproof insulation boards of the embodiment and the comparative example.

[0117] Thermal conductivity determination: refer to GB / T10294-2008 "Determination of steady-state thermal resistance and related properties of insulation materials - Guarded hot plate method".

[0118] Compressive strength determination: refer to GB / T5486-2008 "Test methods for inorganic rigid thermal insulation products".

[0119] The test results are shown in Table 1 below.

[0120] Table 1 Test results

[0121]

[0122] As can be seen from Table 1, in the modified porous microspheres of the present invention, epoxy resin is used as the main component of the basic structure, and phosphate is used as a binder to cure the epoxy resin and enhance the structural stability. Carbamate decomposes and releases gas under heating conditions. These gases produce tiny bubbles in the mixture and expand under the action of heat, prompting the raw material mixture to form porous structure microspheres. At the same time, the phosphate forms a shell structure in the outer layer of the porous structure microspheres. Due to the presence of the shell, it can not only increase the hardness of the modified porous microsphere particles and improve the high temperature resistance, but also block water from entering the modified porous microspheres, thereby effectively reducing the open porosity and water absorption of the modified porous microspheres. Therefore, heat conduction can be effectively reduced and the thermal insulation performance of the fireproof insulation board can be improved; the silane coupling agent can effectively reduce the interfacial energy between the modified porous microspheres and the matrix material, reduce the penetration of harmful substances such as water molecules and oxygen, thereby improving the weather resistance and durability of the fireproof insulation board. 3-Aminopropyltrimethoxysilane undergoes a hydrolysis reaction in the modified porous microspheres, in which three methoxy groups react with water to generate three methanol molecules and three hydroxyl groups. After hydrolysis, the amino and hydroxyl parts in the amino silicone oil can form chemical bonds or hydrogen bonds with functional groups such as silicon or hydroxyl groups in the base material of the fireproof insulation board, thereby forming adhesion between the surfaces, improving the compatibility between the modified porous microspheres and other preparation raw materials of the fireproof insulation board, and greatly improving the mechanical strength of the insulation board.

[0123] Example 4 replaces 3-aminopropyltrimethoxysilane with dimethoxymethylethyldioxysilane. Compared with Example 1, dimethoxymethylethyldioxysilane is not as strong as 3-aminopropyltrimethoxysilane when it is combined with the matrix material after modifying the modified porous microspheres. As a result, the mechanical properties of the fireproof insulation board finally prepared are slightly reduced. Example 5 replaces 3-aminopropyltrimethoxysilane with 3-(methoxy)propyltriethoxysilane. Compared with Example 1, 3-(methoxy)propyltriethoxysilane is not as strong as 3-aminopropyltrimethoxysilane when it is combined with the matrix material after modifying the modified porous microspheres. As a result, the mechanical properties of the fireproof insulation board finally prepared are slightly reduced, and the reinforcing effect on the matrix material is not as good as Example 1. In Example 6, 3-aminopropyltrimethoxysilane was replaced with 3-aminopropyltriethoxysilane. Compared with Example 1, the modified porous microspheres with 3-aminopropyltriethoxysilane may have lower reactivity due to the strong hydrophilicity of the ethoxy group, which results in a slight decrease in the mechanical properties of the fireproof insulation board prepared, and the reinforcing effect on the base material is not as good as that in Example 1.

[0124] In comparative example 1, the silane coupling agent is replaced with trimethoxysilane. Since trimethoxysilane does not contain amino groups, it cannot form chemical bonds or hydrogen bonds with functional groups such as silicon or hydroxyl groups in the base material of the fireproof insulation board, thereby failing to achieve adhesion between the surfaces and failing to improve the overall performance of the fireproof insulation board.

[0125] In comparative example 2, carbamate is replaced with sodium bicarbonate. Under heating conditions, carbamate decomposes to release ammonia, carbon dioxide and water. The release of ammonia will increase the alkalinity of the environment because ammonia is partially decomposed into ammonia water in water, which increases the alkalinity of the solution. Under pure alkaline conditions, the solidification of phosphate is promoted, and the gas produced by the decomposition of sodium bicarbonate may not be enough to achieve the same effect, resulting in insufficient formation of the shell structure, thereby affecting the structural stability and high temperature resistance of the modified porous microspheres.

[0126] In Comparative Example 3, phosphate is replaced by sodium phosphite. Under heating conditions, phosphite exhibits weaker acidity and is inferior to phosphate in terms of curing and bonding, resulting in insufficient formation of the shell structure, thereby affecting the structural stability and high temperature resistance of the modified porous microspheres.

[0127] The present invention is not limited to the above-mentioned embodiments, and various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A fireproof insulation board, characterized in that: The preparation raw materials include: silicate cement, fly ash, silane coupling agent and modified porous microspheres; The raw materials for preparing the modified porous microspheres include epoxy resin, phosphate and carbamate.

2. The fireproof insulation board according to claim 1, characterized in that: The fireproof heat-insulating board comprises the following raw materials in parts by weight: 140-180 parts of silicate cement, 40-90 parts of fly ash, 25-30 parts of modified porous microspheres, and 4-6 parts of silane coupling agent.

3. The fireproof insulation board according to claim 1, characterized in that: The fireproof heat-insulating board is prepared by raw materials further comprising: a water reducing agent and water.

4. The fireproof insulation board according to claim 1, characterized in that: The modified porous microspheres include the following raw materials in parts by weight: 100 to 800 parts of epoxy resin, 300 to 600 parts of phosphate and 10 to 16 parts of carbamate.

5. A method for preparing a fireproof and heat-insulating board as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: S1: mixing the silane coupling agent and the modified porous microspheres, and then adding the silicate cement and pulverized coal to obtain a mixture; S2: Place the mixture in the formwork, and after pouring, demoulding and curing, a fireproof insulation board is obtained.

6. The method for preparing the fireproof heat-insulating board according to claim 5, characterized in that: The preparation method of the modified porous microspheres comprises: A1. Mixing epoxy resin, curing agent and urethane to obtain a mixed solution; A2. dropping the mixture in step A1 into the phosphate solution, stirring and solidifying to obtain particles; A3. Separate the particles and heat them.

7. The method for preparing the fireproof heat-insulating board according to claim 6, characterized in that: The heating temperature is 200-700°C.

8. The method for preparing the fireproof and heat-insulating board according to claim 6, characterized in that: The heating time is 1 to 2 hours.

9. Use of the fireproof and heat-insulating board according to any one of claims 1 to 4 in building wall panels.

10. The use according to claim 9, characterized in that: The building wall panels include a building exterior wall thermal insulation and fireproofing layer or a building interior partition panel.

Citation Information

Patent Citations

  • Heat barrier coating with low heat conductivity and oxidation resistance

    CN110079183A

  • High-water-loss plugging agent solid-phase plugging particles for drilling fluid

    CN111849433A

  • Environment-friendly fireproof insulation board and preparation method thereof

    CN115594468A