High-flow-state early-strength low-shrinkage semi-flexible pavement grouting material and preparation method thereof
By using semi-flexible pavement grouting materials made of cement, oily polyurethane and other raw materials, it solves the problem of difficulty in balancing high flow state, early strength and low shrinkage in the existing technology, and achieves high fluidity, early high strength and low shrinkage. efficiency, improved pavement durability and construction efficiency, and complied with Chinese engineering construction standards.
Patent Information
- Application Number
- CN202410800652.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing semi-flexible pavement grouting materials to take into account the technical problems of high flow state, early strength type and low shrinkage, resulting in slow development of pavement strength, long maintenance time, large shrinkage and prone to cracking.
Semi-flexible pavement grouting material made of raw materials such as cement, oily polyurethane, fly ash, mineral powder, river sand, water reducing agent, retardant, defoaming agent and cellulose. Through a specific mixing and stirring process, it ensures The grouting material has high flow state, early strength type and low shrinkage characteristics.
It achieves high fluidity, early high strength and low shrinkage of the grouting material, can quickly reach the compressive strength and flexural strength, avoid road deformation and disease, conforms to the technical requirements of the China Engineering Construction Standardization Association, and improves construction efficiency and economy. benefit.
Smart Images

Figure BDA0004903277140000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road construction materials, relates to a road grouting material, and specifically relates to a high-fluidity, early-strength, low-shrinkage, semi-flexible road grouting material and a preparation method thereof. Background Art
[0002] Semi-flexible pavement is a new type of composite pavement formed by pouring cement slurry on the basis of asphalt pavement structure. The emergence of semi-flexible pavement successfully combines the advantages of asphalt pavement and cement pavement, and overcomes the shortcomings of both. Compared with asphalt mixtures, semi-flexible pavement materials enhance the ability to resist pavement deformation. On the other hand, compared with cement concrete, semi-flexible pavement materials reduce their modulus and reduce the possibility of cracks. At the same time, it also improves the driving comfort of drivers and the durability of pavement use, and can reduce the damage to the pavement caused by loads. In addition, semi-flexible pavement also resists the erosion of oil pollution, and there is no need to design expansion joints. Semi-flexible roads have the above-mentioned excellent properties, so they are particularly suitable for use in places such as highway toll stations, highway rest areas, uphill sections of roads, and traffic lights on urban roads, which can reduce rutting and wave deformation.
[0003] However, there are still some problems with semi-flexible pavements. The cement grouting materials commonly used in the market for semi-flexible pavements do not solve the problems of slow pavement strength development, long maintenance time, large shrinkage, and easy cracking. They can only be used on some designated roads and cannot be paved on a large area. Therefore, it is very necessary to design a semi-flexible grouting material with high fluidity, early strength, and low shrinkage.
[0004] There are still some problems with the semi-flexible pavement cement-based grouting materials currently available:
[0005] The Chinese invention patent with application publication number CN111943614A discloses a grouting material specially used for semi-flexible pavement, its preparation method and application. This grouting material is composed of key ingredients such as sulphoaluminate cement, microbeads, water reducer, defoamer, color paste and water. Under specific technical conditions, the grouting material exhibits excellent homogeneity, reaching or exceeding 33%, and after 3 hours of curing, its compressive strength is at least 13MPa and its flexural strength is at least 2.8MPa. When the curing time is extended to 7 days, its compressive strength can be increased to at least 36MPa, and its flexural strength is at least 5MPa. This unique formula effectively improves the homogeneity and early strength of the grouting material, providing strong support for the construction of semi-flexible pavements. However, its actual anti-shrinkage effect is not ideal, and the grouting material is prone to cracks during the road use stage.
[0006] The Chinese invention patent with application publication number CN116514483A discloses a self-compacting, high-toughness semi-flexible pavement grouting material and preparation method. It uses tailings sand, phosphogypsum, cement, rubber particles, interface agent, redispersible latex powder, white sugar and water. Its tensile strength grade reaches M30, and it can fill the gaps in the asphalt mixture matrix autonomously under the action of gravity; at the same time, it has high viscosity and seamlessly bonds with the asphalt mixture matrix; there is no shrinkage phenomenon after hardening, supporting the matrix skeleton, and effectively avoiding the deformation of semi-flexible pavement. However, its early mechanical strength is low, and it requires a long hydration time before the strength reaches the standard, resulting in the road surface being unable to be quickly opened to traffic after grouting. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high-fluidity, early-strength, low-shrinkage semi-flexible pavement grouting material and a preparation method, so as to solve the technical problem that the semi-flexible pavement grouting material in the prior art is difficult to have high fluidity, early strength and low shrinkage.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0009] A semi-flexible pavement grouting material is prepared from the following raw materials: cement, oily polyurethane, fly ash, mineral powder, river sand, water reducing agent, retarder, defoaming agent, cellulose and water.
[0010] The cement is made of ordinary silicate cement and sulphoaluminate cement.
[0011] Specifically, the invention is made of the following raw materials, by weight: 500 parts of cement, 15-30 parts of oily polyurethane, 25-50 parts of fly ash, 15-50 parts of mineral powder, 200-350 parts of river sand, 1-3 parts of water reducer, 0.2-0.8 parts of retarder, 0.1-0.3 parts of defoamer, 4-8 parts of cellulose and 200-300 parts of water.
[0012] Preferably, it is made of the following raw materials, measured by weight: 500 parts of cement, 20-30 parts of oily polyurethane, 25-30 parts of fly ash, 25-45 parts of mineral powder, 300-350 parts of river sand, 2-3 parts of water reducer, 0.8 parts of retarder, 0.1-0.2 parts of defoamer, 5-8 parts of cellulose, and 250-300 parts of water.
[0013] Preferably, the cement is made from the following raw materials, measured in parts by weight: 150-200 parts of ordinary Portland cement and 300-350 parts of sulphoaluminate cement.
[0014] Preferably, the river sand is fine aggregate river sand, and the fine aggregate river sand is divided into four particle sizes, namely 40-79 mesh, 80-119 mesh, 120-159 mesh and 160-200 mesh.
[0015] Preferably, the water reducer is a naphthalene-based high-efficiency water reducer, an amino-based high-efficiency water reducer or a polycarboxylic acid high-performance water reducer.
[0016] Preferably, the retarder is one or a combination of more than one of sodium gluconate and sodium citrate.
[0017] Preferably, the defoaming agent is fatty alcohol ester or polysiloxane.
[0018] Preferably, the cellulose is one or a combination of more than one of sodium carboxymethyl cellulose and hydroxypropyl methyl cellulose.
[0019] The present invention also protects a method for preparing the semi-flexible pavement grouting material as described above, the method comprising the following steps: uniformly mixing ordinary Portland cement, sulphoaluminate cement, fly ash, mineral powder, water reducer, retarder and defoamer; adding water, stirring at a speed of 60 r / min for 120 seconds, switching to a speed of 120 r / min for stirring for 30 seconds, and pausing the mixer; adding river sand, and after the river sand is added, starting the mixer, stirring at a speed of 120 r / min for 120 seconds; finally, adding oily polyurethane and stirring at a speed of 120 r / min for 15 seconds to obtain the semi-flexible pavement grouting material.
[0020] Compared with the prior art, the present invention has the following technical effects:
[0021] (I) The present invention is the first to combine ordinary Portland cement, sulphoaluminate cement and oily polyurethane to work together. Sulphoaluminate cement provides the main early strength, ordinary Portland cement ensures the later hydration process, ensuring that the subsequent strength of the grouting material will not decrease, and the oily polyurethane further improves the strength and hardness, making the grouting material more durable. The oily polyurethane has better adhesion, which can ensure the close bonding between the grouting material and the asphalt mixture, thereby improving the stability of the overall structure.
[0022] (II) The semi-flexible pavement grouting material of the present invention has the characteristics of high fluidity, early strength and low shrinkage. The semi-flexible pavement grouting material provided by the present invention has a 1d compressive strength of up to 32MPa, a 1d flexural strength of up to 5.0MPa, a 28d compressive strength of up to 45MPa, a flexural strength of up to 6.0MPa, an initial fluidity of no more than 14s, and a 30min fluidity of no more than 15s. It has the advantages of early strength, fast hardening and high fluidity, and has a low shrinkage rate, good bonding performance, and excellent bonding performance at the contact interface with the asphalt mixture. It can achieve seamless bonding with the asphalt mixture, thereby effectively avoiding the occurrence of diseases such as cracking and deformation of the semi-flexible pavement, and improving the durability and service life of the semi-flexible pavement.
[0023] (III) The semi-flexible pavement grouting material prepared by the present invention fully complies with the standard of the China Association for Engineering Construction Standardization "Technical Specifications for Grouting Semi-flexible Pavements of Urban Roads" (T / CECS1016-2022), and is efficient and convenient to construct, cost-effective, and has excellent road performance, and has broad promotion prospects and application value.
[0024] (IV) The present invention can reduce resource waste and environmental pollution by recycling waste such as fly ash. The "ball effect" of fly ash can further improve the fluidity and strength of the grouting material, making the grouting material have better performance and achieving good economic and environmental benefits.
[0025] (V) The preparation method of the present invention is simple and easy to operate, which reduces the construction difficulty and cost and improves the construction efficiency.
[0026] The specific contents of the present invention are further explained in detail below in conjunction with embodiments. DETAILED DESCRIPTION
[0027] It should be noted that the raw materials in the present invention, unless otherwise specified, are all raw materials known in the prior art. For example, the oily polyurethane, polycarboxylic acid high-performance water-reducing agent and polysiloxane are all commercially available oily polyurethane, polycarboxylic acid high-performance water-reducing agent and polysiloxane.
[0028] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0029] Embodiment 1:
[0030] The present embodiment provides a semi-flexible pavement grouting material, which is made of the following raw materials, by weight: 150 parts of ordinary Portland cement, 350 parts of sulphoaluminate cement, 20 parts of oily polyurethane, 25 parts of fly ash, 25 parts of mineral powder, 300 parts of river sand, 2 parts of water reducer, 0.8 parts of retarder, 0.1 parts of defoamer, 5 parts of cellulose, and 250 parts of water.
[0031] Ordinary Portland cement is ordinary 52.5 grade Portland cement.
[0032] The number average molecular weight of the oily polyurethane is 37000; the oily polyurethane is semi-solid and has a relatively high solid content, which is above 50%.
[0033] The fly ash is special grade fly ash.
[0034] The mineral powder is S95 grade mineral powder
[0035] River sand is fine aggregate river sand, which is divided into four particle sizes, among which the weight ratio is 40-79 mesh: 80-119 mesh: 120-159 mesh: 160-200 mesh = 200:50:25:25.
[0036] The water reducing agent is a polycarboxylic acid high performance water reducing agent.
[0037] The retarder is a mixture of sodium gluconate and sodium citrate, with 0.6 parts of sodium gluconate and 0.2 parts of sodium citrate.
[0038] The defoamer is a fatty alcohol ester.
[0039] The cellulose is sodium carboxymethyl cellulose.
[0040] The present invention also protects a method for preparing a semi-flexible pavement grouting material, the method comprising the following steps:
[0041] Mix ordinary Portland cement, sulphoaluminate cement, fly ash, mineral powder, water reducer, retarder and defoamer evenly; add water, stir at a speed of 60r / min for 120s, switch to a speed of 120r / min and stir for 30s, and pause the mixer; add river sand, and after the river sand is added, start the mixer and stir at a speed of 120r / min for 120s; finally, add oily polyurethane and stir at a speed of 120r / min for 15s to obtain a semi-flexible pavement grouting material.
[0042] According to the "Test Code for Cement and Cement Concrete in Highway Engineering" (JTG E30-2005), the test results of various technical performances of this embodiment are shown in Table 1. It is measured that the initial fluidity of the semi-flexible pavement grouting material of this embodiment is 11.1s, the fluidity after 30 minutes is 14.8s, the shrinkage rate is 0.014%, the 1-day compressive strength is 35.4MPa, the 1-day flexural strength is 6.6MPa, the 28-day compressive strength is 47.7MPa, and the flexural strength is 7.6MPa.
[0043] Embodiment 2:
[0044] The present embodiment provides a semi-flexible pavement grouting material, which is made of the following raw materials, by weight: 200 parts of ordinary Portland cement, 300 parts of sulphoaluminate cement, 20 parts of oily polyurethane, 30 parts of fly ash, 25 parts of mineral powder, 300 parts of river sand, 2 parts of water reducer, 0.8 parts of retarder, 0.1 parts of defoamer, 5 parts of cellulose, and 250 parts of water.
[0045] The types and specifications of the raw materials in this embodiment are the same as those in Embodiment 1.
[0046] The preparation method of the semi-flexible pavement grouting material in this embodiment is the same as the preparation method in Example 1.
[0047] According to the "Test Code for Cement and Cement Concrete in Highway Engineering" (JTG E30-2005), the test results of various technical performances of this embodiment are shown in Table 1. It is measured that the initial fluidity of the semi-flexible pavement grouting material of this embodiment is 10.2s, the fluidity after 30min is 14.0s, the shrinkage rate is 0.012%, the 1-day compressive strength is 32.7MPa, the 1-day flexural strength is 6.1MPa, the 28-day compressive strength is 49.1MPa, and the flexural strength is 7.6MPa.
[0048] Embodiment 3:
[0049] The present embodiment provides a semi-flexible pavement grouting material, which is made of the following raw materials, by weight: 150 parts of ordinary Portland cement, 350 parts of sulphoaluminate cement, 30 parts of oily polyurethane, 25 parts of fly ash, 25 parts of mineral powder, 300 parts of river sand, 3 parts of water reducer, 0.8 parts of retarder, 0.1 parts of defoamer, 5 parts of cellulose, and 250 parts of water.
[0050] The types and specifications of the raw materials in this embodiment are the same as those in Embodiment 1.
[0051] The preparation method of the semi-flexible pavement grouting material in this embodiment is the same as the preparation method in Example 1.
[0052] According to the "Test Code for Cement and Cement Concrete in Highway Engineering" (JTG E30-2005), the test results of various technical performances of this embodiment are shown in Table 1. The initial fluidity of the semi-flexible pavement grouting material of this embodiment is 13.1s, the fluidity after 30 minutes is 14.9s, the shrinkage rate is 0.018%, the 1-day compressive strength is 35.7MPa, the 1-day flexural strength is 7.1MPa, the 28-day compressive strength is 52.4MPa, and the flexural strength is 8.7MPa.
[0053] Embodiment 4:
[0054] The present embodiment provides a semi-flexible pavement grouting material, which is made of the following raw materials, by weight: 150 parts of ordinary Portland cement, 350 parts of sulphoaluminate cement, 20 parts of oily polyurethane, 25 parts of fly ash, 25 parts of mineral powder, 350 parts of river sand, 2 parts of water reducer, 0.8 parts of retarder, 0.1 parts of defoamer, 5 parts of cellulose, and 250 parts of water.
[0055] In this embodiment:
[0056] River sand is fine aggregate river sand, which is divided into four particle sizes, among which the weight ratio is 40-79 mesh: 80-119 mesh: 120-159 mesh: 160-200 mesh = 225:75:25:25.
[0057] The retarder is sodium gluconate.
[0058] The types and specifications of the remaining raw materials in this embodiment are the same as those in Embodiment 1.
[0059] The preparation method of the semi-flexible pavement grouting material in this embodiment is the same as the preparation method in Example 1.
[0060] According to the "Test Code for Cement and Cement Concrete in Highway Engineering" (JTG E30-2005), the test results of various technical performances of this embodiment are shown in Table 1. It is measured that the initial fluidity of the semi-flexible pavement grouting material of this embodiment is 12.7s, the fluidity after 30min is 14.5s, the shrinkage rate is 0.009%, the 1-day compressive strength is 34.6MPa, the 1-day flexural strength is 6.4MPa, the 28-day compressive strength is 48.4MPa, and the flexural strength is 7.6MPa.
[0061] Embodiment 5:
[0062] The present embodiment provides a semi-flexible pavement grouting material, which is made of the following raw materials, by weight: 150 parts of ordinary Portland cement, 350 parts of sulphoaluminate cement, 20 parts of oily polyurethane, 25 parts of fly ash, 25 parts of mineral powder, 300 parts of river sand, 2 parts of water reducer, 0.8 parts of retarder, 0.2 parts of defoamer, 5 parts of cellulose, and 300 parts of water.
[0063] The types and specifications of the raw materials in this embodiment are the same as those in Embodiment 1.
[0064] The preparation method of the semi-flexible pavement grouting material in this embodiment is the same as the preparation method in Example 1.
[0065] According to the "Test Code for Cement and Cement Concrete in Highway Engineering" (JTG E30-2005), the test results of various technical performances of this embodiment are shown in Table 1. It is measured that the initial fluidity of the semi-flexible pavement grouting material of this embodiment is 10.3s, the fluidity after 30min is 13.3s, the shrinkage rate is 0.018%, the 1-day compressive strength is 33.3MPa, the 1-day flexural strength is 5.3MPa, the 28-day compressive strength is 45.1MPa, and the flexural strength is 6.1MPa.
[0066] Embodiment 6:
[0067] The present embodiment provides a semi-flexible pavement grouting material, which is made of the following raw materials, by weight: 150 parts of ordinary Portland cement, 350 parts of sulphoaluminate cement, 20 parts of oily polyurethane, 25 parts of fly ash, 45 parts of mineral powder, 300 parts of river sand, 2 parts of water reducer, 0.8 parts of retarder, 0.1 parts of defoamer, 8 parts of cellulose, and 250 parts of water.
[0068] In this embodiment:
[0069] The cellulose is a mixture of sodium carboxymethylcellulose and hydroxypropyl methylcellulose, wherein the sodium carboxymethylcellulose is 4 parts and the hydroxypropyl methylcellulose is 4 parts.
[0070] The types and specifications of the remaining raw materials in this embodiment are the same as those in Embodiment 1.
[0071] The preparation method of the semi-flexible pavement grouting material in this embodiment is the same as the preparation method in Example 1.
[0072] According to the "Test Code for Cement and Cement Concrete in Highway Engineering" (JTG E30-2005), the test results of various technical performances of this embodiment are shown in Table 1. The initial fluidity of the semi-flexible pavement grouting material of this embodiment is 13.8s, the fluidity after 30min is 14.8s, the shrinkage rate is 0.013%, the 1-day compressive strength is 35.3MPa, the 1-day flexural strength is 5.0MPa, the 28-day compressive strength is 48.0MPa, and the flexural strength is 7.1MPa.
[0073] Table 1 Technical performance test results
[0074]
[0075] In summary: the semi-flexible pavement grouting material of the present invention, under conventional maintenance conditions, has a 1d compressive strength of up to 32MPa, a 1d flexural strength of up to 5.0MPa, a 28d compressive strength of up to 45MPa, and a flexural strength of up to 6.0MPa, an initial fluidity of no more than 14s, and a 30min fluidity of no more than 15s, which meets the technical requirements of the China Association for Engineering Construction Standardization "Technical Specifications for Grouting Semi-flexible Pavements for Urban Roads" (T / CECS1016-2022), and can fill the gaps in the asphalt mixture matrix autonomously by self-leveling under the action of gravity; at the same time, the grouting material has high viscosity and can be seamlessly bonded to the asphalt mixture matrix, effectively avoiding the occurrence of deformation diseases of the semi-flexible pavement. In addition, the grouting material of the present invention has good on-site pouring uniformity, is simple to prepare, and is easy to operate, which can improve construction efficiency, ensure project quality, and realize rapid road opening.
Claims
1. A semi-flexible pavement grouting material, characterized in that: Made of the following raw materials: cement, oily polyurethane, fly ash, mineral powder, river sand, water reducer, retarder, defoamer, cellulose and water; The cement is made of ordinary silicate cement and sulphoaluminate cement.
2. The semi-flexible pavement grouting material according to claim 1, characterized in that: The invention is made of the following raw materials in parts by weight: 500 parts of cement, 15-30 parts of oily polyurethane, 25-50 parts of fly ash, 15-50 parts of mineral powder, 200-350 parts of river sand, 1-3 parts of water reducer, 0.2-0.8 parts of retarder, 0.1-0.3 parts of defoamer, 4-8 parts of cellulose and 200-300 parts of water.
3. The semi-flexible pavement grouting material according to claim 2, characterized in that: The invention is made of the following raw materials in parts by weight: 500 parts of cement, 20-30 parts of oily polyurethane, 25-30 parts of fly ash, 25-45 parts of mineral powder, 300-350 parts of river sand, 2-3 parts of water reducer, 0.8 parts of retarder, 0.1-0.2 parts of defoamer, 5-8 parts of cellulose and 250-300 parts of water.
4. The semi-flexible pavement grouting material according to claim 1, characterized in that: The cement is made from the following raw materials, measured in parts by weight: 150-200 parts of ordinary Portland cement and 300-350 parts of sulphoaluminate cement.
5. The semi-flexible pavement grouting material according to claim 1, characterized in that: River sand is fine aggregate river sand, which is divided into four particle sizes, namely 40-79 mesh, 80-119 mesh, 120-159 mesh and 160-200 mesh.
6. The semi-flexible pavement grouting material according to claim 1, characterized in that: The water reducer is a naphthalene-based high-efficiency water reducer, an amino-based high-efficiency water reducer or a polycarboxylic acid high-performance water reducer.
7. The semi-flexible pavement grouting material according to claim 1, characterized in that: The retarder is one or a combination of more than one of sodium gluconate and sodium citrate.
8. The semi-flexible pavement grouting material according to claim 1, characterized in that: The defoamer is fatty alcohol ester or polysiloxane.
9. The semi-flexible pavement grouting material according to claim 1, characterized in that: The cellulose is one or a combination of more than one of sodium carboxymethyl cellulose and hydroxypropyl methyl cellulose.
10. A method for preparing a semi-flexible pavement grouting material according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: uniformly mixing ordinary Portland cement, sulphoaluminate cement, fly ash, mineral powder, water reducing agent, retarder and defoamer; adding water, stirring at a speed of 60 r / min for 120 seconds, switching to a speed of 120 r / min for stirring for 30 seconds, and pausing the mixer; adding river sand, and after the river sand is added, starting the mixer, stirring at a speed of 120 r / min for 120 seconds; finally, adding oily polyurethane, stirring at a speed of 120 r / min for 15 seconds, and obtaining a semi-flexible pavement grouting material.
Citation Information
Patent Citations
Polyurethane modified epoxy resin grouting material
CN102417337A
Plate bottom grouting material for fabricated cement concrete pavement plate
CN113105198A