Preparation method and application of low-dielectric-constant multi-composite microwave dielectric ceramic
By preparing low dielectric constant multiple composite microwave dielectric ceramics, the problem of insufficient performance of existing ceramics in high-frequency applications is solved, the lightweight and high quality factor of the ceramics are achieved, and the antenna design is suitable for the new generation of communication technology and meets the requirements of environmental protection and cost-effectiveness requirements.
Patent Information
- Application Number
- CN202410901940.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing microwave dielectric ceramics have problems such as insufficient performance, high cost, and poor environmental protection in high-frequency applications, making it difficult to meet the needs of new generation communication technologies such as 5G and 6G.
A method for preparing low dielectric constant multiple composite microwave dielectric ceramics is adopted, and [(Zn0. 8Mg0.2)1-xNix]2SiO4 ceramics utilize the mixed phase structure of olivine and willemite to optimize process parameters to lower the sintering temperature and improve the quality factor.
Significantly lowers the sintering temperature, improves the microwave dielectric properties of ceramics, including relative dielectric constant and quality factor, and enhances water absorption resistance. It is suitable for miniaturization and lightweight antenna design in 5G and 6G wireless communication technologies to meet the requirements of future communication equipment. need.
Smart Images

Figure CN118724575A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of ceramic material preparation, and in particular to a preparation method and application of a low dielectric constant multiple composite microwave dielectric ceramic. Background Art
[0002] Microwave dielectric ceramics, as an indispensable dielectric material in microwave frequency band circuits, play a vital role in the field of wireless communications with their unique properties. This type of ceramic material has significant characteristics such as high dielectric constant, low loss and near-zero frequency temperature coefficient, which makes it widely used in microwave circuits such as resonators, filters, and dielectric antennas. Microwave dielectric ceramics are classified in various ways and can be divided from multiple angles such as composition, structure, dielectric properties, and application frequency domain. In particular, according to the application frequency domain, it can be divided into several major categories such as low frequency (0.8~4GHz), medium frequency (4~8GHz) and high frequency. Each type of ceramic material has its own unique dielectric properties and application scenarios. In terms of preparation technology, microwave dielectric ceramics cover a variety of methods such as powder preparation technology. These technologies are crucial to controlling the microstructure and properties of ceramics, and directly affect the performance of ceramics in microwave circuits. By optimizing the preparation process, the performance of microwave dielectric ceramics can be further improved to meet the growing market demand.
[0003] In the field of modern communications, microwave dielectric ceramics are widely used in mobile phones, car phones, TV satellite receivers and other equipment. With the continuous development of wireless communication technology, the application prospects of microwave dielectric ceramics will be broader. In the future, with the popularization of new generation communication technologies such as 5G and 6G, microwave dielectric ceramics will play a greater role in higher frequency bands and more complex application scenarios. At the same time, the development of microwave dielectric ceramics also faces some challenges. With the growing market demand for high performance, low cost, and environmental protection, microwave dielectric ceramics need to continue to innovate and improve.
[0004] The continuous emergence of new preparation technologies and material design methods has brought new opportunities for the development of microwave dielectric ceramics. The performance and competitiveness of microwave dielectric ceramics can be further improved by continuously developing new materials, optimizing preparation processes, and reducing production costs. In summary, microwave dielectric ceramics, as an important electronic material, play an irreplaceable role in the field of wireless communications. With the continuous advancement of technology and the continuous growth of market demand, microwave dielectric ceramics will usher in a broader development space and application prospects. We have reason to believe that in the near future, microwave dielectric ceramics will play a more important role in the field of wireless communications and create a better life for mankind. Summary of the invention
[0005] The technical problem to be solved by the present application is to overcome the defects in the prior art and provide a preparation method and application of low dielectric constant multiple composite microwave dielectric ceramics.
[0006] This application adopts the following technical solutions to solve the above technical problems:
[0007] A method for preparing a low dielectric constant multi-composite microwave dielectric ceramic comprises the following steps:
[0008] (1) After mixing the main agent, water is added and ball milled to obtain a mixture;
[0009] (2) drying, calcining and cooling the mixed material obtained in step (1) to obtain a prefabricated material;
[0010] (3) performing secondary ball milling, sintering, and secondary cooling on the prefabricated material to obtain a composite ceramic material;
[0011] Wherein, the main agent is composed of zinc oxide, magnesium oxide, nickel monoxide and silicon dioxide.
[0012] Preferably, step (1) satisfies at least one of the following conditions:
[0013] The time of the first ball milling is 20 to 30 hours, preferably 24 hours.
[0014] The rotation speed of the first ball milling is 300-500 rpm, preferably 450 rpm.
[0015] Preferably, in step (1), the diameter of the mixture is 8 to 15 mm and the thickness is 3 to 6 mm.
[0016] Preferably, at least one of the following conditions is met in step (2):
[0017] The drying time is 20 to 30 hours;
[0018] The drying temperature is 90-100°C;
[0019] The primary cooling is programmed cooling, preferably, the programmed cooling is performed at 4-8°C / min;
[0020] The temperature of the first cooling is cooled to 90-100°C.
[0021] Preferably, the calcination in step (2) satisfies at least one of the following conditions:
[0022] The calcination temperature is 1000-1200°C, preferably 1150°C.
[0023] The calcination time is 2 to 4 hours, preferably 3 hours.
[0024] The calcination is carried out by programmed temperature increase, preferably, the programmed temperature increase is carried out at 4-8°C / min.
[0025] Preferably, the sintering in step (3) satisfies at least one of the following conditions:
[0026] The secondary ball milling time is 20 to 30 hours, preferably 24 hours.
[0027] The rotation speed of the secondary ball milling is 300-500 rpm, preferably 450 rpm;
[0028] The sintering method is programmed temperature increase, preferably, the programmed temperature increase is performed at 4-8°C / min.
[0029] The sintering temperature is 1200-1400°C; preferably 1250-1375°C;
[0030] The sintering temperature is 3 to 6 hours, preferably 4 hours;
[0031] The sintering is performed under air;
[0032] The secondary cooling is programmed cooling, preferably, the programmed cooling is performed at 4-8°C / min;
[0033] The temperature of the secondary cooling is cooled to 90-100°C.
[0034] Preferably, step (3) further includes a grinding operation before the secondary ball milling, and a binder is added during the grinding process, wherein the mass percentage of the binder is 15 to 30 wt%.
[0035] Preferably, the grinding in step (3) is followed by granulation and compression molding;
[0036] Wherein, the granulation screen mesh number is 30 to 50 mesh;
[0037] The pressure of the pressing molding is 100-200 MPa.
[0038] A low dielectric constant multiple composite microwave dielectric ceramic, which is prepared by the above method for preparing low dielectric constant multiple composite microwave dielectric ceramic, wherein the composite ceramic is [(Zn 0.8 Mg 0.2 ) 1-x Ni x ]2SiO4 ceramics, X is 0.05~0.2
[0039] A method for preparing low-dielectric-constant multi-composite microwave dielectric ceramics and its application in dielectric materials and semiconductor devices.
[0040] On the basis of conforming to the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present application.
[0041] The reagents and raw materials used in this application are commercially available.
[0042] The positive effects of this application are:
[0043] (1) The preparation method provided by the present application is compared with single-phase Mg2SiO4 and Zn2SiO4. 0.8 Mg 0.2 ) 1-x Ni x ]2SiO4 ceramics can significantly reduce the sintering temperature. 0.8 Mg 0.2 ) 1-x Ni x ]2SiO4 (x = 0.05), but it is clear that the Q×f values of these ceramics can be significantly improved by replacing Mg and Zn with Ni, accompanied by a significant decrease in the resonant frequency temperature coefficient (τ f ) decreases. As (Zn 0.8 Mg 0.2 ) 2+ As the value of x increases, the unit cell volume gradually decreases, and the average distortion of the oxygen tetrahedron increases accordingly. At the same time, the symmetry of the six-membered ring formed by the shared angles between Zn(1)O4, Zn(2)O4, and SiO4 is enhanced. For x values in the range of 0.05 to 0.2, the Q×f value of the ceramic increases due to the enhanced symmetry of the six-membered ring. The increase in x value leads to the increase of (Zn 0.8 Mg 0.2 ) deviates from the stoichiometric ratio with Ni, thereby increasing the liquid content and reducing the grain size, thereby increasing the Q×f value. When x = 0.2 and the sintering temperature is 1325 ° C, [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 ceramics show the best microwave dielectric properties: relative dielectric constant (ε r ) is 6.84, the quality factor multiplied by the frequency (Q×f) is 27,185GHz, and the resonant frequency temperature coefficient (τ f ) is -37ppm / ℃, which has broad application prospects.
[0044] (2) This application utilizes the mixed phase structure of olivine and willemite, which not only gives the material a low dielectric constant, but also significantly improves its quality factor. By precisely controlling the raw material ratio and synthesis process, [(Zn 0.8 Mg0.2 ) 1- x Ni x ]2SiO4 ceramics, which not only have low density and low dielectric constant, but also have high quality factor, showing excellent comprehensive performance. In terms of application fields, this lightweight silicate microwave dielectric ceramic material has broad application prospects in key components such as dielectric substrates, resonators and filters. Especially in advanced wireless communication technologies such as 5G and 6G, miniaturization and lightweight have become important trends in antenna design. The lightweight microwave dielectric ceramic material of the present invention just meets this demand and provides strong support for the development of wireless communication equipment.
[0045] (3) The ceramic material provided in the present application achieves significant weight reduction of the material and also has excellent resistance to water absorption, thereby ensuring its stability under various environmental conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The present application can be better understood by referring to the description given below in conjunction with the accompanying drawings. The accompanying drawings, together with the following detailed description, are included in this specification and form a part of this specification, and are used to further illustrate the preferred embodiments of the present application and explain the principles and advantages of the present application.
[0047] in:
[0048] Figure 1 The scanning electron microscope images and average grain size images of the ceramic materials prepared in Examples 1 to 4;
[0049] Figure 2 The scanning electron microscope images and average grain size images of the ceramic materials prepared in Comparative Examples 1 to 3;
[0050] Figure 3 XRD patterns of ceramic materials prepared in Examples 1 to 4;
[0051] Figure 4 XRD diagrams of ceramic materials prepared in Comparative Examples 1 to 3; DETAILED DESCRIPTION
[0052] The present application is further described below by way of examples, but the present application is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are selected according to conventional methods and conditions, or according to the product instructions.
[0053] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0054] The raw materials in the following examples are all commercially available.
[0055] Example 1
[0056] [(Zn 0.8 Mg 0.2 ) 0.95 Ni 0.05 ] A method for preparing 2SiO4 microwave dielectric ceramic material, specifically comprising the following steps:
[0057] (1) According to the chemical formula [(Zn 0.8 Mg 0.2 ) 0.95 Ni 0.05 ]2SiO4: Weigh ZnO, MgO, NiO and SiO2 with a purity greater than 99.9%; put them into a nylon jar containing zirconium oxide balls, add 2 / 3 of the bottle of pure deionized water, mix them, and ball-mill them together at 400-450r / min on a ball mill for 24 hours. Put the mixture into an oven and dry it at 95°C for 24 hours;
[0058] (2) placing the dried mixed material in step (1) upside down in a crucible, heating the mixture to 1150° C. at a rate of 5° C. / min for 3 hours, then cooling the mixture to 100° C. at a rate of 5° C. / min and then cooling the mixture naturally to obtain the prefabricated material;
[0059] (3) adding purified deionized water to the preform obtained in step (2) for ball milling at a speed of about 400 to 450 r / min for 24 hours, and drying at 95° C. to obtain a dry preformed powder;
[0060] (4) The prefabricated powder obtained in step (3) was added with 15-30 wt% of PVA binder and ground, and then sieved through a 40-mesh screen to form granules, and then pressed into a cylinder with a diameter of 11 mm and a height of 5.5 mm using a corresponding mold at a pressure of about 150 MPa. The cylinder sample was heated to 500-550°C at a rate of 5°C / min for 4 hours to discharge PVA, and then heated to 1325°C at a rate of 5°C / min and sintered for 4 hours, and then cooled to 100°C at a rate of 5°C / min and then cooled naturally to obtain [(Zn 0.8 Mg 0.2 ) 0.95 Ni 0.05 ]2SiO4 microwave dielectric ceramics.
[0061] This implementation case [(Zn 0.8 Mg 0.2 ) 0.95 Ni 0.05 ]2SiO4 microwave dielectric ceramics were tested by XRD and SEM. Figure 3 Sintered at 1325℃ [(Zn 0.8 Mg 0.2 ) 0.95 Ni0.05 The X-ray diffraction peaks of the [ZnMgNi]2SiO4 microwave dielectric ceramics detected two phases of Zn2SiO4 and MgNi(SiO4). Checking other cases (Zn 1-x Mg x )2SiO4 could not form a solid solution when 0 < X < 0.4. From Figure 1 the SEM image shown in (a), it can be seen that the ceramic grains sintered at 1325 °C are larger in size, have more voids, and the density is 3.90 g / cm 3 , the average grain size is about 15.8 μm, and its dielectric properties are ε r is 6.6, Qxf is 15,005 GHz, τ f is -46 ppm / °C.
[0062] Example 2
[0063] [(Zn 0.8 Mg 0.2 ) 0.9 Ni 0.1 2SiO4 microwave dielectric ceramic material preparation method, specifically including the following steps:
[0064] Steps (2), (3), and (4) are the same as those in Example (1). The difference is that in this example, the chemical formula ratio weighing in step (1) is different. In this example, [(Zn 0.8 Mg 0.2 ) 0.9 Ni 0.1 2SiO4 is weighed;
[0065] The [(Zn 0.8 Mg 0.2 ) 0.9 Ni 0.1 2SiO4 microwave dielectric ceramics of this example are subjected to XRD and SEM tests. From Figure 3 the sintering shown at 1325 °C, the X-ray diffraction peaks of [(Zn 0.8 Mg 0.2 ) 0.9 Ni 0.1 2SiO4 detected two phases of Zn2SiO4 and MgNi(SiO4), indicating that Zn2SiO4 and Mg2SiO4 did not form a solid solution here. As Figure 1 shown in the SEM image of (b), it can be seen that the ceramic sintered at 1325 °C has significantly smaller grain size than that in Example 1, and the density is 3.97 g / cm 3 , the increase in density leads to an increase in the Qxf value. The average grain size is about 5.28 μm, and its dielectric properties are ε r is 6.7, Qxf is 22,370 GHz, τ f is -47 ppm / °C.
[0066] Example 3
[0067] [(Zn 0.8 Mg 0.2 ) 0.85 Ni 0.15 ] A method for preparing 2SiO4 microwave dielectric ceramic material, specifically comprising the following steps:
[0068] Steps (2), (3), and (4) are the same as those in Example (1). The difference is that the chemical formula ratios in step (1) are different. In this case, [(Zn 0.8 Mg 0.2 ) 0.85 Ni 0.15 ]2SiO4 is weighed;
[0069] This implementation case [(Zn 0.8 Mg 0.2 ) 0.85 Ni 0.15 ]2SiO4 microwave dielectric ceramics were tested by XRD and SEM. Figure 3 Sintered at 1325℃ [(Zn 0.8 Mg 0.2 ) 0.85 Ni 0.15 The X-ray diffraction peak of ]2SiO4 detected two phases, Zn2SiO4 and MgNi(SiO4), such as Figure 1 (c) The SEM image shows that the grain size of the ceramic sintered at 1325°C gradually decreases, the voids decrease, and the density increases to 4.0 g / cm 3 The increase in density leads to an increase in the Qxf value. The average grain size is about 4.7 μm, and its dielectric properties are ε r is 6.77, Qxf is 24,171GHz, τ f It is -40ppm / ℃.
[0070] Example 4
[0071] [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ] A method for preparing 2SiO4 microwave dielectric ceramic material, specifically comprising the following steps:
[0072] Steps (2), (3), and (4) are the same as those in Example (1). The difference is that the chemical formula ratios in step (1) are different. In this case, [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 is weighed;
[0073] This implementation case [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 microwave dielectric ceramics were tested by XRD and SEM. Figure 3 Sintered at 1325℃ [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 X-ray diffraction peaks also detected Zn2SiO4 and MgNi(SiO4), such as Figure 1 The SEM image (d) shows that the ceramic sintered at 1325°C has the smallest grain size, fewer voids, and an increased density of 4.1 g / cm 3 The increase in density leads to an increase in the Qxf value, the average grain size is around 2.94μm, and its dielectric properties are ε r is 6.84, Qxf is 27,185GHz, τ f It is -37ppm / ℃.
[0074] Comparative Example 1
[0075] Compared with Example 4, the only difference is that the [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 microwave dielectric ceramic, the other conditions are the same as those in Example 1, and the specific operations are as follows:
[0076] (1) According to the chemical formula [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4: Weigh ZnO, MgO, NiO and SiO2 with a purity greater than 99.9%; put them into a nylon jar containing zirconium oxide balls, add 2 / 3 of the bottle of pure deionized water, mix them, and ball-mill them together at 400-450r / min on a ball mill for 24 hours. Put the mixture into an oven and dry it at 95°C for 24 hours;
[0077] (2) placing the dried mixed material in step (1) upside down in a crucible, heating the mixture to 1150° C. at a rate of 5° C. / min for 3 hours, then cooling the mixture to 100° C. at a rate of 5° C. / min and then cooling the mixture naturally to obtain the prefabricated material;
[0078] (3) adding purified deionized water to the preform obtained in step (2) for ball milling at a speed of about 400 to 450 r / min for 24 hours, and drying at 95° C. to obtain a dry preformed powder;
[0079] (4) The prefabricated powder obtained in step (3) was added with 15-30 wt% of PVA binder for grinding, and then sieved through a 40-mesh screen to form granules, and then pressed into a cylinder with a diameter of 11 mm and a height of 5.5 mm using a corresponding mold at a pressure of about 150 MPa. The cylinder sample was heated to 500-550°C at a rate of 5°C / min for 4 hours to discharge PVA, and then heated to 1300°C at a rate of 5°C / min for 4 hours, and then cooled to 100°C at a rate of 5°C / min and then cooled naturally to obtain [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 microwave dielectric ceramics.
[0080] In this comparative case, [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 microwave dielectric ceramics were tested by XRD and SEM. Figure 4 (a) Sintered at 1300℃ [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 X-ray diffraction peaks also detected Zn2SiO4 and MgNi(SiO4), such as Figure 2 The average grain size of the ceramic obtained in the SEM image (a) is about 4.49 μm, the grains are relatively uniform, and there are fewer voids. Its dielectric properties are εr of 6.82, Qxf of 24,762 GHz, τ f It is -34ppm / ℃.
[0081] Comparative Example 2
[0082] This comparative example is the same as steps (1), (2), and (3) of comparative example 1, except that the sintering temperature in step (4) is different. In this case, the temperature is increased at 5°C / min to 1350°C and sintered for 4 hours.
[0083] In this comparative case, [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 microwave dielectric ceramics were tested by XRD and SEM. Figure 4(b) Sintered at 1350℃ [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 X-ray diffraction peaks also detected Zn2SiO4 and MgNi(SiO4), such as Figure 2 The average grain size of the ceramic obtained in the SEM image (b) is about 9.54 μm. The grain size is enlarged, and its dielectric properties are εr of 6.51, Qxf of 23,700 GHz, τ f It is -26ppm / ℃.
[0084] Comparative Example 3
[0085] The steps (1), (2) and (3) of this comparative example are the same as those of comparative example 1, except that the sintering temperature in step (4) is different. In this case, the temperature is increased at 5°C / min to 1375°C and sintered for 4 hours.
[0086] In this comparative case, [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 microwave dielectric ceramics were tested by XRD and SEM. Figure 4 (c) Sintered at 1375℃ [(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4 X-ray diffraction peaks also detected Zn2SiO4 and MgNi(SiO4), such as Figure 2 The average grain size of the ceramic obtained in the SEM image (c) is about 9.79 μm. The grains gradually grow larger, and the dielectric properties tend to decrease with temperature. Its dielectric property is ε r is 6.48, Qxf is 14,966 GHz, τ f It is -31 ppm / ℃.
[0087] Effect Example 1
[0088] Table 1 shows the dielectric properties and other parameter information of implementation cases 1 to 4 and comparative cases 1 to 3 for easy reference as shown below:
[0089] Ingredients Sintering temperature(℃) <![CDATA[Density (g / cm 3 )]]> <![CDATA[ε r ]]> Qxf(GHZ) <![CDATA[d av (μm)]]> Example 1 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.95 Ni 0.05 ]2SiO4]]> 1325 3.90 6.60 15,005 15.84 Example 2 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.9 Ni 0.1 ]2SiO4]]> 1325 3.97 6.70 22,370 5.28 Example 3 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.85 Ni 0.15 ]2SiO4]]> 1325 4.00 6.77 24,762 4.47 Example 4 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4]]> 1325 4.10 6.84 27,185 2.94 Comparative Example 1 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4]]> 1300 4.06 6.82 24,762 4.49 Comparative Example 2 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4]]> 1350 4.00 6.51 23,700 9.54 Comparative Example 3 <![CDATA[[(Zn 0.8 Mg 0.2 ) 0.8 Ni 0.2 ]2SiO4]]> 1375 3.97 6.48 14,966 9.79
[0090] from Figure 1 It can be seen that when x=0.05, the abnormal growth of grains in Comparative Example 1 is obvious, and the grain size distribution is uneven. With the increase of Ni, the abnormal growth of grains decreases, and the grain size becomes more uniform. Figure 1From the average grain size graph, it can be seen that as the particle size distribution range increases, the particle size distribution is normally distributed. When x = 0.05, the average particle size decreases from 15.84μm to 5.28μm (x = 0.1), 4.47μm (x = 0.15) and 2.94μm (x = 0.2). This is because (Zn 0.8 Mg 0.2 ) decreases, and the Ni content during sintering also increases, which accelerates the diffusion of atoms during sintering and makes its composition more uniform.
[0091] from Figure 1 It can be seen that the grain size of the ceramic is [(Zn 0.8 Mg 0.2 ) 1-x Ni x ]2SiO4 (x=0.05, 0.1, 0.15, 0.2) shows that the size gradually decreases with the increase of x. Examples 3 and 4 are smaller in size, more uniform, and have better performance.
[0092] Finally, it should be noted that in this application, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements that are not explicitly listed, or also includes elements that are inherent to such process, method, article or apparatus.
[0093] Although the present application has been disclosed above through the description of the specific embodiments of the present application, it should be understood that those skilled in the art can design various modifications, improvements or equivalents to the present application within the spirit and scope of the attached scheme. These modifications, improvements or equivalents should also be considered to be included in the scope of protection claimed in the present application.
Claims
1. A method for preparing a low dielectric constant multi-composite microwave dielectric ceramic, characterized in that: The steps include: (1) After mixing the main agent, water is added and ball milled to obtain a mixture; (2) drying, calcining and cooling the mixed material obtained in step (1) to obtain a prefabricated material; (3) performing secondary ball milling, sintering, and secondary cooling on the prefabricated material to obtain a composite ceramic material; Wherein, the main agent is composed of zinc oxide, magnesium oxide, nickel monoxide and silicon dioxide.
2. The method for preparing the low dielectric constant multi-composite microwave dielectric ceramic according to claim 1, characterized in that: Step (1) satisfies at least one of the following conditions: The time of the first ball milling is 20 to 30 hours, preferably 24 hours. The rotation speed of the first ball milling is 300-500 rpm, preferably 450 rpm.
3. The method for preparing the low dielectric constant multi-composite microwave dielectric ceramic according to claim 1, characterized in that: In step (1), the diameter of the mixture is 8 to 15 mm and the thickness is 3 to 6 mm.
4. The method for preparing the low dielectric constant multi-composite microwave dielectric ceramic according to claim 1, characterized in that: At least one of the following conditions is met in step (2): The drying time is 20 to 30 hours; The drying temperature is 90-100°C; The primary cooling is programmed cooling, preferably, the programmed cooling is performed at 4-8°C / min; The temperature of the first cooling is cooled to 90-100°C.
5. The method for preparing the low dielectric constant multi-composite microwave dielectric ceramic according to claim 1, characterized in that: The calcination in step (2) satisfies at least one of the following conditions: The calcination temperature is 1000-1200°C, preferably 1150°C. The calcination time is 2 to 4 hours, preferably 3 hours. The calcination is carried out by programmed temperature increase, preferably, the programmed temperature increase is carried out at 4-8°C / min.
6. The method for preparing the low dielectric constant multiple composite microwave dielectric ceramic according to claim 1, characterized in that: The sintering in step (3) satisfies at least one of the following conditions: The secondary ball milling time is 20 to 30 hours, preferably 24 hours. The rotation speed of the secondary ball milling is 300-500 rpm, preferably 450 rpm; The sintering method is programmed temperature increase, preferably, the programmed temperature increase is performed at 4-8°C / min. The sintering temperature is 1200-1400°C; preferably 1250-1375°C; The sintering temperature is 3 to 6 hours, preferably 4 hours; The sintering is performed under air; The secondary cooling is programmed cooling, preferably, the programmed cooling is performed at 4-8°C / min; The temperature of the secondary cooling is cooled to 90-100°C.
7. The method for preparing low dielectric constant multiple composite microwave dielectric ceramics according to claim 1, characterized in that: Step (3) also includes a grinding operation before the secondary ball milling, and a binder is added during the grinding process, wherein the mass percentage of the binder is 15 to 30 wt%.
8. The method for preparing the low dielectric constant multiple composite microwave dielectric ceramic according to claim 7, characterized in that: Step (3) of granulating and pressing after grinding; Wherein, the granulation screen mesh number is 30 to 50 mesh; The pressure of the pressing molding is 100-200 MPa.
9. A low dielectric constant multiple composite microwave dielectric ceramic, which is prepared by the preparation method of low dielectric constant multiple composite microwave dielectric ceramic according to any one of claims 1 to 8, wherein: The low dielectric constant composite microwave dielectric ceramic is [(Zn 0.8 Mg 0.2 ) 1-x Ni x ]2SiO4 ceramics, X is 0.05~0.
2.
10. A method for preparing the low dielectric constant multi-composite microwave dielectric ceramic according to claim 9, and its application in dielectric materials and semiconductor devices.
Citation Information
Patent Citations
Preparation method of microwave dielectric ceramic material and dielectric ceramic block
CN111377731A