Low-temperature sintered PZT-based piezoelectric ceramic material as well as preparation method and application thereof
By using nano-scale multi-element glass powder as a sintering aid, the problem of PZT ceramics sintering at low temperatures is solved, and a PZT ceramic material with high density and excellent electrical properties is achieved, which is suitable for multi-layer laminated piezoelectric ceramic components. Reduced production costs.
Patent Information
- Application Number
- CN202410773066.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-17
AI Technical Summary
It is difficult to sinter PZT-based piezoelectric ceramic materials at temperatures below 900°C with the existing technology, resulting in stoichiometric deviation and decrease in electrical properties, and traditional sintering aids will affect the density and electrical properties of ceramics.
Nanoscale PbO-B2O3-SiO2-Li2O-Bi2O3-CuO glass powder is used as a sintering aid and is prepared by the sol-gel method to form a glass phase to reduce the sintering temperature and accelerate diffusion and mass transfer between ceramic substrates through liquid phase sintering. process, combined with appropriate amounts of CuO and Bi2O3 to reduce the impact on ceramic properties.
It is possible to sinter PZT ceramics at a temperature below 900°C, maintaining high density and excellent electrical properties, meeting the application needs of multi-layer laminated piezoelectric ceramic components, and reducing production costs.
Smart Images

Figure BDA0004894713310000091 
Figure BDA0004894713310000092 
Figure BDA0004894713310000093
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of piezoelectric ceramic materials, and in particular relates to a low-temperature sintered PZT-based piezoelectric ceramic material and a preparation method and application thereof. Background Art
[0002] In recent years, due to the large-scale use of piezoelectric actuators and transformers, high-power piezoelectric ceramic materials have attracted extensive research and attention. In order to obtain high power density, multi-layer stacked piezoelectric ceramic components have gradually become a recent research hotspot. Stacked devices represented by piezoelectric actuators have special requirements for the performance of piezoelectric materials, generally higher piezoelectric constants, electromechanical coupling coefficients, dielectric constants, and lower losses. PMN-PZT piezoelectric ceramics have high piezoelectric constants, high stability and density, and moderate dielectric losses. They are suitable for multi-layer stacked piezoelectric ceramic components and have broad application prospects, which have attracted great attention from researchers.
[0003] However, the sintering temperature of PMN-PZT piezoelectric ceramics is as high as 1260℃. During high-temperature sintering, PbO volatilizes severely, resulting in a shift in the stoichiometric ratio and a decrease in the electrical properties of the ceramics. In addition, the current laminated structure tends to use Ag-Pd precious metals with higher melting points as internal electrodes for multi-layer stacking and one-time sintering, but such laminated devices are expensive. If PZT piezoelectric ceramics can be sintered below 900℃, Ag can be used as the internal electrode, which can not only reduce costs but also inhibit the volatilization of PbO.
[0004] Liquid phase sintering is the most common and economical method to achieve low-temperature sintering of piezoelectric ceramics. At present, the research hotspots of low-temperature sintering aids mainly include low-melting glass materials and low-melting compounds, among which oxides such as ZnO, Bi2O3, Li2CO3, and B2O3 are often used as sintering aids. One mechanism for this type of oxide to reduce the sintering temperature is to distort the lattice, reduce the potential barrier between electric domains, and accelerate ion diffusion, but it will seriously deteriorate the performance of piezoelectric ceramics; the other is to produce a low-melting liquid phase through low-melting glass\oxides or form a solid solution with the substances in the piezoelectric ceramics, but the temperature for forming the liquid phase is often above 900°C, which cannot be achieved at a lower sintering temperature, and the piezoelectric ceramics will inevitably introduce excess second phases after the final sintering, affecting the electrical properties of the piezoelectric ceramics. Therefore, how to circumvent the shortcomings of the above-mentioned methods and develop a PZT-based piezoelectric ceramic material that takes into account both low sintering temperature and excellent electrical properties is a technical difficulty in this field. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a low-temperature sintered PZT-based piezoelectric ceramic material and its preparation method and application in view of the deficiencies in the prior art. The material can be sintered at a temperature below 900°C, has a high density after sintering, has excellent electrical properties, and meets the application requirements of piezoelectric ceramic components.
[0006] In order to solve the technical problem proposed by the present invention, the present invention provides a low-temperature sintered PZT-based piezoelectric ceramic material, the chemical composition of which is 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3+a%LBPBSC, wherein LBPBSC is nano-scale PbO-B2O3-SiO2-Li2O-Bi2O3-CuO glass powder, and the molar ratio of PbO, B2O3, SiO2, Li2O, Bi2O3, and CuO in LBPBSC is (35-40):(10-15):(5-8):(10-15):(10-12):(5-10), and the mass of LBPBSC is 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )a% of O3 mass, 0.5≤a≤0.6.
[0007] In the above scheme, the preparation method of the LBPBSC comprises the following steps:
[0008] 1) dissolving lithium acetate, bismuth acetate, copper acetate, lead acetate, boric acid and silicon acetate in anhydrous ethanol respectively, heating and stirring to form a sol;
[0009] 2) mixing and stirring the sols of each group to form a mixed sol, and drying to obtain a xerogel;
[0010] 3) The dry gel is heat-treated in a muffle furnace to obtain LBPBSC.
[0011] Furthermore, the heating and stirring temperature is 40 to 50° C., and the stirring time is 1 to 3 hours.
[0012] Furthermore, the drying temperature is 60-80°C.
[0013] Furthermore, the temperature of the heat treatment is 450-550°C.
[0014] Furthermore, the particle size of the LBPBSC is 200-300 nm.
[0015] The present invention also provides a method for preparing a low temperature sintered PZT-based piezoelectric ceramic material, which specifically comprises the following steps:
[0016] S1, according to the chemical composition 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3 PbO, MgO, Nb2O5, ZrO2 and TiO2 are weighed, ball-milled and mixed evenly, dried, sieved, the mixed powder is pressed into blocks, pre-fired in a muffle furnace, ball-milled into powder, and dried to obtain a PZT-based piezoelectric ceramic matrix powder;
[0017] S2, ball-milling the ceramic matrix powder and LBPBSC, drying, and sieving to obtain low-temperature sintered PZT-based piezoelectric ceramic powder;
[0018] S3, adding a binder to the low-temperature sintered PZT-based piezoelectric ceramic powder and molding it, sintering it after debinding, polishing the sintered ceramic, coating it with silver paste, and polarizing it after calcination to obtain a low-temperature sintered PZT-based piezoelectric ceramic material.
[0019] In the above scheme, in step S1, the ball milling mixing time is 24 to 48 hours.
[0020] In the above scheme, in step S1, the sieving is through a 80-100 mesh sieve.
[0021] In the above scheme, the pre-firing temperature is 900-950°C and the pre-firing time is 2-4 hours. When the pre-firing temperature is too low or the pre-firing time is too short, the solid phase reaction between the powders is insufficient, the reaction is not complete, or even no solid phase reaction occurs, which seriously reduces the performance of the piezoelectric ceramics; when the pre-firing temperature is too high or the pre-firing time is too long, the PbO in the ceramic matrix volatilizes violently, resulting in a deviation in the stoichiometric ratio, which is not conducive to the regulation of the ceramic matrix composition.
[0022] In the above solution, the particle size of the PZT-based piezoelectric ceramic matrix powder is 0.5 to 1 μm.
[0023] In the above scheme, in step S2, the ball milling mixing time is 24 to 48 hours.
[0024] In the above solution, the particle size of the low-temperature sintered PZT-based piezoelectric ceramic powder is less than 1 μm.
[0025] In the above scheme, the binder is a PVA solution with a mass fraction of 5 to 15%.
[0026] In the above solution, the added amount of the binder is 0.3-0.5% of the mass of the low-temperature sintered PZT-based piezoelectric ceramic powder.
[0027] In the above scheme, the molding process is first granulation and then pressing, and the pressing pressure is 10-20MPa.
[0028] In the above scheme, the debinding temperature is 500-600°C, the heating rate is 1-2°C / min, and the debinding time is 2-4h.
[0029] In the above scheme, the sintering temperature is 850-900° C. and the sintering time is 2-4 hours.
[0030] In the above scheme, the calcination temperature is 650-730° C., and the calcination time is 0.5-1 h.
[0031] In the above scheme, the polarization is carried out in silicone oil at 120-140° C., the polarization electric field strength is 3-3.5 kV / mm, and the polarization time is 20-30 min.
[0032] The present invention also provides an application of a low-temperature sintered PZT-based piezoelectric ceramic material, which is used to prepare piezoelectric ceramic components.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1) The present invention is directed to PZT ceramic matrix 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6)O3, developed a specific sintering aid LBPBSC suitable for the matrix, LBPBSC is a nano-scale multi-component glass powder prepared by the sol-gel method, can form a glass phase at a lower temperature, added to the PZT ceramic matrix, uniformly dispersed between the pores of the PZT ceramic particles, forming a capillary effect, and through liquid phase sintering to accelerate the diffusion and mass transfer process between the ceramic matrix, forming a synergistic effect, to achieve the purpose of significantly reducing the sintering temperature of the PZT ceramic; the PZT ceramic matrix in the present invention is a typical soft piezoelectric ceramic, in order to minimize the elements in the glass powder to dope the powder "hard", the main raw materials of the glass are set to PbO and SiO2, while ensuring that the glass phase can be formed to minimize the impact on the PZT matrix, while introducing Cu, Bi, B, Li to adjust The softening temperature of glass powder can be controlled, and the introduction of "hard" doping elements can be reduced as much as possible; among them, the Pb in LBPBSC is consistent with the basic powder of PZT ceramics, which can minimize the impact on the electrical properties of piezoelectric ceramics; CuO and Bi2O3 can not only produce liquid phase by themselves, but also form a low eutectic liquid phase with PbO in PZT, which can greatly reduce the use of sintering aids; B2O3 has a small ion radius and good cooling performance. When the content is relatively small, it is not easy to replace with the ions of the main crystal phase, which can enable PZT ceramics to maintain high piezoelectric properties; SiO2 plays the role of a network former in glass, which is conducive to the formation of amorphous glass; Li2O is a network exosome, which can make the glass structure loose, reduce the softening temperature of glass, and form a glass phase at a lower temperature.
[0035] 2) The PZT-based piezoelectric ceramic material of the present invention can be sintered at a temperature below 900°C. The X-ray diffraction (XRD) test confirms that the synthesized product has a single perovskite structure; the scanning electron microscope (SEM) test confirms that the piezoelectric ceramic sintered at a low temperature has a high density and a uniform grain size. The PZT-based piezoelectric ceramic material of the present invention also has excellent electrical properties and a large piezoelectric constant (d 33 ≥500Pc / N), and a large dielectric coupling coefficient (Kp≥0.6). Therefore, the PZT-based piezoelectric ceramic material of the present invention fully meets the application requirements of LTCC technology and multi-layer laminated piezoelectric ceramic components. When applied to multi-layer piezoelectric ceramic components, silver electrodes can be used to replace expensive silver-palladium electrodes, thereby reducing production costs and effectively avoiding the diffusion of silver elements, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the XRD pattern of the low temperature sintered PZT-based piezoelectric ceramic material prepared in Example 1 of the present invention.
[0037] Figure 2This is a SEM image of the low-temperature sintered PZT-based piezoelectric ceramic material prepared in Example 1 of the present invention.
[0038] Figure 3 The SEM image and EDS element distribution diagram of the cross-section of the stacked driver prepared in Application Example 1 of the present invention, wherein (a), (b), (c), and (d) are SEM images of the cross-section of the stacked driver, and (e), (f), (g), and (h) are distribution diagrams of Ag, Ti, Zr, and Pb elements in the cross-section area of Figure (d), respectively. DETAILED DESCRIPTION
[0039] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0040] In the following examples, the purity of PbO, MgO, Nb2O5, ZrO2 and TiO2 used is above 99%; the lithium acetate, bismuth acetate, copper acetate, lead acetate, boric acid and silicon acetate used are all analytical grade (AR).
[0041] Example 1
[0042] The low temperature sintered PZT-based piezoelectric ceramic material in this embodiment has the following chemical composition:
[0043] 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3+0.5%LBPBSC,
[0044] The LBPBSC is a nano-scale PbO-B2O3-SiO2-Li2O-Bi2O3-CuO glass powder, and the molar ratio of PbO, B2O3, SiO2, Li2O, Bi2O3 and CuO in the LBPBSC is 35:10:5:10:10:5. The preparation method of the LBPBSC comprises the following steps:
[0045] 1) Dissolve lithium acetate, bismuth acetate, copper acetate, lead acetate, boric acid, and silicon acetate in anhydrous ethanol respectively, and stir at 50°C for 1 h using a magnetic stirrer to form a sol;
[0046] 2) mixing and stirring the sols of each group to form a mixed sol, and drying at 80° C. to obtain a dry gel;
[0047] 3) The dry gel is heat treated at 500° C. in a muffle furnace to obtain LBPBSC with a particle size of 200 nm. The method for preparing the low temperature sintered PZT-based piezoelectric ceramic material in this embodiment comprises the following steps:
[0048] S1, according to the chemical composition 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3 PbO, MgO, Nb2O5, ZrO2 and TiO2 were weighed, ball-milled and mixed for 24 hours, dried, and passed through an 80-mesh sieve. The mixed powder was pressed into blocks, kept at 950°C in a muffle furnace for 4 hours, and then ball-milled into powder, dried, to obtain a PZT-based piezoelectric ceramic matrix powder with a particle size of 0.5 to 1 μm;
[0049] S2, ball-milling the ceramic matrix powder and 0.5% of the mass of the ceramic matrix powder by LBPBSC for 24 hours, drying, and sieving to obtain low-temperature sintered PZT-based piezoelectric ceramic powder with a particle size of <1 μm; the ball milling process in steps S1 and S2 is: using deionized water as solvent, zirconia balls as ball milling media, the mass ratio of material, balls and water is 1:1.5:1, and the ball milling speed is 100 r / min;
[0050] S3, adding a 5% PVA solution by mass to the low-temperature sintered PZT-based piezoelectric ceramic powder, the amount of PVA solution added is 0.3% of the mass of the low-temperature sintered PZT-based piezoelectric ceramic powder, granulating, and then pressing into a ceramic sheet with a diameter of 19 mm and a thickness of 1 mm, heating the ceramic sheet to 600°C at a rate of 1°C / min and keeping it for 2 hours to remove the binder, and then keeping it at 850°C for 4 hours to sinter it into porcelain, polishing the sintered ceramic, coating it with silver paste, calcining at 650 for 0.5 hours, and polarizing it in silicone oil at 120°C with a polarization electric field strength of 3 kV / mm and a polarization time of 30 minutes, cleaning and aging for 24 hours, to obtain a low-temperature sintered PZT-based piezoelectric ceramic material.
[0051] Figure 1 This is the XRD diagram of the low-temperature sintered PZT-based piezoelectric ceramic material prepared in this embodiment. It can be seen from the figure that the position and relative intensity of each diffraction peak of the synthetic product are consistent with the standard JCPDS card (88-1867) of PZT, indicating that the synthetic product has a single perovskite structure.
[0052] Figure 2 This is an SEM image of the low-temperature sintered PZT-based piezoelectric ceramic material prepared in this embodiment. It can be seen from the figure that the ceramic grains are tightly combined, the density is high, the grain size distribution is uniform, and the grain size is 0.8 to 1.2 μm, which is beneficial to the movement of domain walls in the piezoelectric ceramic and the improvement of piezoelectric properties.
[0053] Application Example 1
[0054] The low temperature sintered PZT-based piezoelectric ceramic material in Example 1 is made into a stacked actuator, which specifically includes the following steps:
[0055] S1, according to the chemical composition 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3 PbO, MgO, Nb2O5, ZrO2 and TiO2 were weighed, ball-milled and mixed for 24 hours, dried, and passed through an 80-mesh sieve. The mixed powder was pressed into blocks, kept at 950°C in a muffle furnace for 4 hours, and then ball-milled into powder, dried, to obtain a PZT-based piezoelectric ceramic matrix powder with a particle size of 0.5 to 1 μm;
[0056] S2, ball-milling the ceramic matrix powder and 0.5% of the mass of the ceramic matrix powder by LBPBSC for 24 hours, drying, and sieving to obtain low-temperature sintered PZT-based piezoelectric ceramic powder with a particle size of <1 μm; the ball milling process in steps S1 and S2 is: using deionized water as solvent, zirconia balls as ball milling media, the mass ratio of material, balls and water is 1:1.5:1, and the ball milling speed is 100 r / min;
[0057] S3, anhydrous ethanol and butanone are mixed in a mass ratio of 7:3 as a solvent (addition amount 96g), triethyl phosphate (7g) as a dispersant, polyvinyl butyral PVB (20g) and phthalate (3g) as a binder, and a low-temperature sintered PZT-based piezoelectric ceramic powder (100g) are used to prepare a slurry. After the slurry is defoamed, it is cast into a ceramic film, and the inner electrode silver paste is brushed on the ceramic film, and then stacked to form a green body, and the temperature is increased to 600℃ at a rate of 1℃ / min and kept for 2h to remove the binder, and then sintered at 850℃ for 4h. The sintered laminated ceramics are polished and brushed with external electrode silver paste. After calcination at 650 for 0.5h, it is polarized in silicone oil at 120℃ with a polarization electric field strength of 3kV / mm and a polarization time of 30min. After cleaning and aging for 24h, a laminated driver is obtained.
[0058] The prepared laminated driver was polished and the SEM image and EDS element distribution map of the laminated driver section were obtained. Figure 3 As shown in the figure, the boundary between the piezoelectric ceramic layer and the inner electrode layer is obvious, the thickness between the layers is relatively uniform, and the overall structure is relatively regular, without defects such as stratification; the grain size in the ceramic layer is uniform, the microstructure is relatively dense, and there are no large numbers of closed pores. This result shows that the multilayer piezoelectric ceramic driver is well sintered at 850°C. In addition, it can be seen from Figure (e) that the inner electrode layer has strong continuity, and the Ag element is concentrated in the electrode layer without obvious diffusion to the ceramic layer, indicating that the laminated driver has a complete structure and good conductivity, verifying that the low-temperature sintered PZT-based piezoelectric ceramic material of the present invention can meet the application requirements of multilayer laminated piezoelectric ceramic components.
[0059] Example 2
[0060] The low temperature sintered PZT-based piezoelectric ceramic material in this embodiment has the following chemical composition:
[0061] 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3+0.55%LBPBSC,
[0062] Wherein, LBPBSC is nano-scale PbO-B2O3-SiO2-Li2O-Bi2O3-CuO glass powder, and the molar ratio of PbO, B2O3, SiO2, Li2O, Bi2O3 and CuO in LBPBSC is 37:12:6:12:11:7; the preparation method of LBPBSC comprises the following steps:
[0063] 1) Dissolve lithium acetate, bismuth acetate, copper acetate, lead acetate, boric acid, and silicon acetate in anhydrous ethanol respectively, and stir at 40°C for 2 h using a magnetic stirrer to form a sol;
[0064] 2) mixing and stirring the sols of each group to form a mixed sol, and drying at 60° C. to obtain a xerogel;
[0065] 3) The dry gel is heat treated at 450° C. in a muffle furnace to obtain LBPBSC with a particle size of 230 nm. The method for preparing the low temperature sintered PZT-based piezoelectric ceramic material in this embodiment comprises the following steps:
[0066] S1, according to the chemical composition 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3 PbO, MgO, Nb2O5, ZrO2 and TiO2 were weighed, ball-milled and mixed for 36 hours, dried, and passed through a 90-mesh sieve. The mixed powder was pressed into blocks, kept at 900°C in a muffle furnace for 2 hours, ball-milled into powder, and dried to obtain a PZT-based piezoelectric ceramic matrix powder with a particle size of 0.5 to 1 μm;
[0067] S2, ball-milling the ceramic matrix powder and 0.55% of the mass of the ceramic matrix powder with LBPBSC for 36 hours, drying, and sieving to obtain low-temperature sintered PZT-based piezoelectric ceramic powder with a particle size of <1 μm; the ball milling process in steps S1 and S2 is: using deionized water as the solvent, zirconia balls as the ball milling medium, the mass ratio of material, ball and water is 1:1.5:1, and the ball milling speed is 100 r / min;
[0068] S3, adding a 10% PVA solution by mass to the low-temperature sintered PZT-based piezoelectric ceramic powder, the amount of the PVA solution added is 0.4% of the mass of the low-temperature sintered PZT-based piezoelectric ceramic powder, granulating, and then pressing into a ceramic sheet with a diameter of 19 mm and a thickness of 1 mm, heating the ceramic sheet to 550°C at a rate of 1.5°C / min and keeping it for 3 hours to remove the binder, and then keeping it at 875°C for 2 hours to sinter it into porcelain, polishing the sintered ceramic, coating it with silver paste, calcining it at 700°C for 0.75 hours, and polarizing it in silicone oil at 130°C with a polarization electric field strength of 3.2 kV / mm, polarizing for 20 minutes, cleaning and aging for 24 hours, to obtain a low-temperature sintered PZT-based piezoelectric ceramic material;
[0069] Example 3
[0070] The low temperature sintered PZT-based piezoelectric ceramic material in this embodiment has the following chemical composition:
[0071] 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3+0.6%LBPBSC,
[0072] Wherein, LBPBSC is nano-scale PbO-B2O3-SiO2-Li2O-Bi2O3-CuO glass powder, and the molar ratio of PbO, B2O3, SiO2, Li2O, Bi2O3 and CuO in LBPBSC is 40:15:8:15:12:10; the preparation method of LBPBSC comprises the following steps:
[0073] 1) Dissolve lithium acetate, bismuth acetate, copper acetate, lead acetate, boric acid, and silicon acetate in anhydrous ethanol respectively, and stir at 45°C for 3 hours using a magnetic stirrer to form a sol;
[0074] 2) mixing and stirring the sols of each group to form a mixed sol, and drying at 70° C. to obtain a dry gel;
[0075] 3) The dry gel is heat treated at 550° C. in a muffle furnace to obtain LBPBSC with a particle size of 300 nm. The method for preparing the low temperature sintered PZT-based piezoelectric ceramic material in this embodiment comprises the following steps:
[0076] S1, according to the chemical composition 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6)O3 PbO, MgO, Nb2O5, ZrO2 and TiO2 were weighed, ball-milled and mixed for 48 hours, dried, and passed through a 100-mesh sieve. The mixed powder was pressed into blocks, kept at 925°C in a muffle furnace for 3 hours, and then ball-milled into powder, dried, to obtain a PZT-based piezoelectric ceramic matrix powder with a particle size of 0.5 to 1 μm;
[0077] S2, ball-milling the ceramic matrix powder and 0.6% of the mass of the ceramic matrix powder with LBPBSC for 24 hours, drying, and sieving to obtain low-temperature sintered PZT-based piezoelectric ceramic powder with a particle size of <1 μm; the ball milling process in steps S1 and S2 is: using deionized water as the solvent, zirconia balls as the ball milling medium, the mass ratio of material, ball and water is 1:1.5:1, and the ball milling speed is 100 r / min;
[0078] S3, adding a 15% PVA solution by mass to the low-temperature sintered PZT-based piezoelectric ceramic powder, the amount of the PVA solution added is 0.5% of the mass of the low-temperature sintered PZT-based piezoelectric ceramic powder, granulating, and then pressing into a ceramic sheet with a diameter of 19 mm and a thickness of 1 mm, heating the ceramic sheet to 500°C at a rate of 2°C / min and keeping it for 4 hours to remove the binder, and then sintering it at 850°C for 3 hours to form porcelain, polishing the sintered ceramic, coating it with silver paste, calcining it at 730 for 1 hour, polarizing it in silicone oil at 140°C, the polarization electric field strength is 3.5 kV / mm, the polarization time is 25 minutes, cleaning and aging for 24 hours, and obtaining a low-temperature sintered PZT-based piezoelectric ceramic material;
[0079] Comparative Example 1
[0080] The difference between Comparative Example 1 and Example 1 is only that a=0.4.
[0081] Comparative Example 2
[0082] The difference between Comparative Example 2 and Example 1 is only that a=0.7.
[0083] Comparative Example 3
[0084] The only difference between Comparative Example 3 and Example 1 is that LBPBSC is replaced by a sintering aid prepared by directly mixing PbO, B2O3, SiO2, Li2O, Bi2O3, and CuO in a molar ratio of 35:10:5:10:10:5, and the particle size of the sintering aid is 200 nanometers.
[0085] Comparative Example 4
[0086] The only difference between Comparative Example 4 and Example 1 is that LBPBSC does not contain PbO, and the molar ratios of other components remain unchanged.
[0087] The performance of the low-temperature sintered PZT-based piezoelectric ceramic materials prepared in each embodiment and each comparative example was tested.
[0088] ρ is the volume density, which is tested using the Archimedes drainage method.
[0089] d 33 is the piezoelectric constant, and its formula is:
[0090]
[0091] Where F3 represents the stress applied in the polarization direction; Q3 represents the electric displacement generated on the electrode surface; d 33 is the measured piezoelectric constant, the first 3 in the subscript indicates the polarization direction, and the second 3 indicates the stress direction. 33 The piezoelectric constant was tested by a tester (ZJ-4AN, Institute of Acoustics, Chinese Academy of Sciences).
[0092] ε r is the relative dielectric constant, and its formula is:
[0093]
[0094] In the formula, C represents the capacitance of the ceramic sample, in F; t represents the thickness of the ceramic sample, in m; A represents the effective area of the electrode, in m 2 ; ε0 represents the dielectric constant of vacuum, ε0=8.854×10 -12 (F / m).
[0095] Q m is the mechanical quality factor, and its formula is:
[0096]
[0097] Where C0 represents the static capacitance of the piezoelectric material; C1 represents the equivalent capacitance of the piezoelectric material; C0+C1 is approximately equal to the capacitance of the piezoelectric material measured at 1kHz; R1 represents the minimum impedance at resonance; △f=f a -f r The above parameters are measured by impedance analyzer (1260A+1296A, Solartron Analytical, UK).
[0098] K p is the plane electromechanical coupling coefficient, and its formula is:
[0099]
[0100] In the formula, f r is the resonant frequency; f ais the anti-resonance frequency. To ensure the accuracy of the test results, the diameter / thickness of the test sample of the present invention is greater than 10. The above parameters are measured by an impedance analyzer (1260A+1296A, Solartron Analytical Company, UK).
[0101] Tanδ is the dielectric loss, and its formula is:
[0102]
[0103] In the formula, I R Represents the portion of the current consumed in the dielectric material; I C The dielectric constant and dielectric loss of the material were tested using an impedance analyzer (1260A+1296A, Solartron Analytical, UK) at a test frequency of 1kHz.
[0104] P r For residual polarization intensity, the present invention uses RTI-Multiferroic ferroelectric tester (Radiant Technology Company, USA) to test the ferroelectric properties of piezoelectric ceramics based on Sawyer-Tower circuit to obtain hysteresis loop (PE curve). The test frequency is 1Hz, the test electric field is 30kV / cm, and in order to prevent the edge of the sample and the air from breaking down during the test, the ceramic sample is completely immersed in high boiling point silicone oil.
[0105] T c The Curie temperature is obtained by testing the dielectric constant at different temperatures using a broadband dielectric spectrometer (Novocontrol concept 80).
[0106] Table 1
[0107]
[0108] It can be seen from Table 1 that Examples 1 to 3 have high density and piezoelectric properties; the sintering aids in Comparative Examples 1 and 2 are the same as those in the examples, but the usage amounts exceed the reference values. The amount in Comparative Example 1 is lower than the reference value, and the liquid phase directly or indirectly formed between the sintering aid and the matrix powder during the sintering process cannot fully wet the powder particles, and the ceramic cannot be completely densified. The amount in Comparative Example 2 is higher than the reference value, and too much liquid phase will segregate at the grain boundaries to form a second impurity. Therefore, although the ceramic has an extremely high density, its piezoelectric properties are poor. The sintering aids used in Comparative Examples 3 and 4 are too different from those in the examples, and ideal results cannot be obtained in terms of density and piezoelectric properties.
[0109] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.
Claims
1. A low temperature sintered PZT-based piezoelectric ceramic material, characterized in that: Its chemical composition is 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3+a%LBPBSC, wherein LBPBSC is nano-scale PbO-B2O3-SiO2-Li2O-Bi2O3-CuO glass powder, and the molar ratio of PbO, B2O3, SiO2, Li2O, Bi2O3, and CuO in LBPBSC is (35-40):(10-15):(5-8):(10-15):(10-12):(5-10), and the mass of LBPBSC is 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )a% of O3 mass, 0.5≤a≤0.
6.
2. The low temperature sintered PZT-based piezoelectric ceramic material according to claim 1, characterized in that: The preparation method of the LBPBSC comprises the following steps: 1) dissolving lithium acetate, bismuth acetate, copper acetate, lead acetate, boric acid and silicon acetate in anhydrous ethanol respectively, heating and stirring to form a sol; 2) mixing and stirring the sols of each group to form a mixed sol, and drying to obtain a xerogel; 3) The dry gel is heat-treated in a muffle furnace to obtain LBPBSC.
3. The low temperature sintered PZT-based piezoelectric ceramic material according to claim 2, characterized in that: The heating and stirring temperature is 40-50° C., and the stirring time is 1-3 hours; the drying temperature is 60-80° C.; the heat treatment temperature is 450-550° C.; and the particle size of the LBPBSC is 200-300 nm.
4. A method for preparing a low temperature sintered PZT-based piezoelectric ceramic material as claimed in claim 1, characterized in that: The following steps are involved: S1, according to the chemical composition 0.38Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.62Pb(Zr 0.4 Ti 0.6 )O3 PbO, MgO, Nb2O5, ZrO2 and TiO2 are weighed, ball-milled and mixed evenly, dried, sieved, the mixed powder is pressed into blocks, pre-fired in a muffle furnace, ball-milled into powder, and dried to obtain a PZT-based piezoelectric ceramic matrix powder; S2, ball-milling the ceramic matrix powder and LBPBSC, drying, and sieving to obtain low-temperature sintered PZT-based piezoelectric ceramic powder; S3, adding a binder to the low-temperature sintered PZT-based piezoelectric ceramic powder and molding it, sintering it after debinding, polishing the sintered ceramic, coating it with silver paste, and polarizing it after calcination to obtain a low-temperature sintered PZT-based piezoelectric ceramic material.
5. The method for preparing a low temperature sintered PZT-based piezoelectric ceramic material according to claim 4, characterized in that: The sintering temperature is 850-900° C., and the sintering time is 2-4 hours.
6. The method for preparing a low temperature sintered PZT-based piezoelectric ceramic material according to claim 4, characterized in that: In step S1, the ball milling mixing time is 24 to 48 hours, and the sieving is through an 80-100 mesh sieve; the pre-firing temperature is 900 to 950° C., and the pre-firing time is 2 to 4 hours; and the particle size of the PZT-based piezoelectric ceramic matrix powder is 0.5 to 1 μm.
7. The method for preparing a low temperature sintered PZT-based piezoelectric ceramic material according to claim 4, characterized in that: In step S2, the ball milling mixing time is 24 to 48 hours; and the particle size of the low-temperature sintered PZT-based piezoelectric ceramic powder is less than 1 μm.
8. The method for preparing a low temperature sintered PZT-based piezoelectric ceramic material according to claim 4, characterized in that: The binder is a PVA solution with a mass fraction of 5-15%, and the added amount of the binder is 0.3-0.5% of the mass of the low-temperature sintered PZT-based piezoelectric ceramic powder; the molding process is granulation first and then pressing, and the pressing pressure is 10-20MPa.
9. The method for preparing a low temperature sintered PZT-based piezoelectric ceramic material according to claim 4, characterized in that: The debinding temperature is 500-600°C, the heating rate is 1-2°C / min, and the debinding time is 2-4h; the calcination temperature is 650-730°C, and the calcination time is 0.5-1h; the polarization is carried out in silicone oil at 120-140°C, the polarization electric field strength is 3-3.5kV / mm, and the polarization time is 20-30min.
10. Use of the low-temperature sintered PZT-based piezoelectric ceramic material according to claim 1 in preparing piezoelectric ceramic components.
Citation Information
Patent Citations
Method for preparing low-melting-point quarternary BZBS (BaO-ZnO-B2O3-SiO2) glass by virtue of sol-gel method
CN105439419A
Low-temperature sintering method of lead zirconate titanate-based piezoelectric ceramic piece
CN107573067A
Piezoelectric ceramic low-temperature co-fired sintering agent and preparation method thereof
CN113402285A
Production of inorganic glass and inorganic glass
JP1999001326A
Method of manufacturing nano-glass powder for low temperature sintering
KR100813601B1