Ceramic body and method for producing same
By using a specific proportion of SiC powder and the firing and impregnation process, a Si-impregnated SiC ceramic body with high thermal conductivity is formed, which solves the problem of improving the thermal conductivity of the ceramic body and achieves high-efficiency performance of the ceramic body in applications such as heat exchangers.
Patent Information
- Application Number
- CN202410274641.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to stably improve the thermal conductivity of ceramic bodies composed of Si-impregnated SiC with existing technology, affecting its performance in applications such as heat exchangers.
By using a molding material containing SiC powder with an average particle diameter D50 of 15 to 50 μm and 2 to 8 μm in a mass ratio of 3:7 to 7:3, and performing sintering and impregnation processes, a SiC skeleton portion and metal with a high filling density are formed. Ceramic body of Si impregnated part.
Significantly improves the thermal conductivity of the ceramic body to more than 140W/mK, improving the heat recovery of the heat exchanger and the thermal conductivity of other ceramic bodies.
Smart Images

Figure CN118724593A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to ceramic bodies and methods for making the same. Background Art
[0002] In recent years, there is a demand for improving the fuel consumption of automobiles. In particular, in order to prevent the deterioration of fuel economy when the engine is cooled, such as when the engine is started, a system is expected to preheat the cooling water, engine oil, automatic transmission fluid (ATF: Automatic Transmission Fluid) and the like to reduce friction losses. In addition, a system is expected to heat the catalyst for exhaust gas purification in order to pre-activate the catalyst.
[0003] In the above-mentioned system, a heat exchanger having a honeycomb shape and a ceramic body (honeycomb structure) composed of Si impregnated SiC is used (Patent Document 1). The ceramic body is manufactured by degreasing a ceramic molded body containing silicon carbide (hereinafter referred to as "SiC") and then impregnating it with metallic silicon (hereinafter referred to as "Si").
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6763699 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In recent years, in order to improve the performance of heat exchangers (for example, to improve heat recovery performance, etc.), it has been required to improve the thermal conductivity of a ceramic body composed of Si-impregnated SiC.
[0009] SiC constitutes the skeleton of the ceramic body and has a higher thermal conductivity than Si. Therefore, it is considered that the thermal conductivity of the ceramic body can be increased by increasing the proportion of SiC in the ceramic body.
[0010] However, in the conventional methods, it is difficult to stably increase the proportion of SiC in the ceramic body (frame part), and there is a problem that the thermal conductivity of the ceramic body cannot be fully improved. It should be noted that, in the above, the ceramic body used for heat exchangers is used as an example, but there is also a demand for improving the thermal conductivity of ceramic bodies other than heat exchangers.
[0011] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a ceramic body having a high thermal conductivity and composed of Si-impregnated SiC, and a method for producing the same.
[0012] The present inventors have conducted intensive research on a ceramic body composed of Si impregnated SiC, and have found that the above-mentioned problems can be solved by using a molding material containing two types of SiC powders having a predetermined average particle size D50 in a predetermined ratio, thereby completing the present invention. That is, the present invention is exemplified as follows.
[0013] [1] A method for manufacturing a ceramic body, comprising a molding step and a firing and impregnation step; in the molding step, a molding material containing SiC powder having an average particle size D50 of 15 to 50 μm and SiC powder having an average particle size D50 of 2 to 8 μm in a mass ratio of 3:7 to 7:3 is molded to obtain a molded body; in the firing and impregnation step, the molded body is fired and impregnated with metal Si.
[0014] [2] The method for producing a ceramic body according to [1], wherein the firing and impregnation steps are performed by firing the molded body while it is in contact with metal Si.
[0015] [3] The method for producing a ceramic body according to [2], wherein the sintering is performed at a temperature of 1400 to 1600° C. in an inert gas atmosphere or in a vacuum.
[0016] [4] The method for producing a ceramic body according to any one of [1] to [3], wherein the ceramic raw material contained in the molding material is only the SiC powder.
[0017] [5] The method for manufacturing a ceramic body according to any one of [1] to [4], wherein the molded body is subjected to at least one of a drying treatment and a degreasing treatment between the molding step and the firing and impregnation step.
[0018] [6] A method for manufacturing a ceramic body according to any one of [1] to [5], wherein the molded body has a honeycomb shape or a hollow honeycomb shape; the honeycomb shape is a shape having an outer peripheral wall and a plurality of partition walls arranged on the inner side of the outer peripheral wall and dividing the plurality of cells extending from the first end face to the second end face; the hollow honeycomb shape is a shape having an inner peripheral wall, an outer peripheral wall, and a plurality of partition walls arranged between the inner peripheral wall and the outer peripheral wall and dividing the plurality of cells extending from the first end face to the second end face.
[0019] [7] A ceramic body comprising: a SiC skeleton portion containing SiC particles having a particle size of 15 to 50 μm and SiC particles having a particle size of 2 to 8 μm in a volume ratio of 3:7 to 7:3; and a metal Si impregnation portion formed around at least a portion of the SiC skeleton portion.
[0020] It should be noted that, since silicon has properties similar to those of metals, it is generally treated as a metal in the art and is referred to as "metal silicon" or "metal Si". Silicon is also used as an example for specific description in the embodiments described below.
[0021] Effects of the Invention
[0022] According to the present invention, it is possible to provide a ceramic body having high thermal conductivity and composed of Si-impregnated SiC, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a partially enlarged cross-sectional view of a molded body produced by the method for producing a ceramic body according to an embodiment of the present invention.
[0024] Figure 2 This is a cross-sectional view of a honeycomb-shaped molded body taken along a direction perpendicular to the cell extending direction.
[0025] Figure 3 This is a cross-sectional view of a molded body having a hollow honeycomb shape, taken at right angles to the cell extending direction.
[0026] Description of Reference Numerals
[0027] 10: formed body, 100: honeycomb formed body, 110: outer peripheral wall, 120: cell, 130: partition wall, 140: inner peripheral wall, 200: hollow honeycomb formed body. DETAILED DESCRIPTION
[0028] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. It should be understood that the present invention is not limited to the following embodiments, and that within the scope of the present invention, based on the common knowledge of those skilled in the art, the following embodiments may be appropriately modified, improved, etc., and also fall within the scope of the present invention.
[0029] (1) Method for manufacturing ceramic body
[0030] The method for producing a ceramic body according to the embodiment of the present invention includes a molding step and a firing and impregnation step. These steps will be described in detail.
[0031] <Molding process>
[0032] The molding step is a step of molding a molding material containing SiC powder having an average particle size D50 of 15 to 50 μm (hereinafter referred to as "SiC powder A") and SiC powder having an average particle size D50 of 2 to 8 μm (hereinafter referred to as "SiC powder B") in a mass ratio of 3:7 to 7:3 to obtain a molded body.
[0033] Here, a partial enlarged cross-sectional view of the molded body produced under the above conditions is shown in FIG. Figure 1 .like Figure 1 As shown, by using two kinds of SiC powders A and B having an average particle size D50 at the above-mentioned mass ratio, in the molded body 10, the SiC powder B having a small average particle size D50 is easily filled between the SiC powders A having a large average particle size D50, thereby being able to increase the packing density of the SiC powders (SiC powders A and B) constituting the molded body 10. As a result, the thermal conductivity of the ceramic body obtained by performing the sintering and impregnation steps on the molded body 10 is improved. On the other hand, if it is not the above-mentioned conditions, the packing density of the SiC particles constituting the molded body cannot be sufficiently increased, and therefore the thermal conductivity of the ceramic body cannot be sufficiently increased.
[0034] Here, the "average particle size D50" of the SiC powders A and B used in the molding step refers to the particle size of the cumulative value 50% (D50) in the particle size distribution determined by a laser primary diffraction-scattering method.
[0035] The SiC powder A may be one kind or two or more kinds thereof may be used in combination. Specifically, two or more kinds of SiC powders A having an average particle size D50 within a range of 15 to 50 μm may be used.
[0036] Similarly, one type of SiC powder B may be used alone, or two or more types may be used in combination. Specifically, two or more types of SiC powder B having an average particle size D50 within a range of 2 to 8 μm may be used.
[0037] From the viewpoint of stably ensuring the above-mentioned effects, the average particle size D50 of SiC powder A is preferably 20 to 45 μm, more preferably 25 to 40 μm. From the viewpoint of stably ensuring the above-mentioned effects, the average particle size D50 of SiC powder B is preferably 3 to 7 μm, more preferably 4 to 6 μm.
[0038] Furthermore, from the viewpoint of stably ensuring the above-mentioned effect, the mass ratio of SiC powder A to SiC powder B is preferably 4:6 to 6:4.
[0039] The molding material preferably contains only SiC powders A and B as ceramic raw materials. SiC powders A and B have high thermal conductivity and a thermal expansion coefficient close to that of metal Si to be impregnated in the step described below, and thus can obtain a ceramic body having excellent resistance to thermal stress.
[0040] Here, the ceramic raw material refers to a raw material that constitutes the skeleton of the ceramic body after the firing and impregnation steps.
[0041] The molding material may contain components known in the art as required. As known components, dispersion medium, adhesive, plasticizer and dispersant etc. may be cited. The content of these components is not particularly limited as long as it does not hinder the effect of the present invention.
[0042] Examples of the dispersion medium include water and a mixed solvent of water and an organic solvent such as alcohol, and water is particularly preferably used.
[0043] Examples of the binder include organic binders such as methylcellulose, hydroxypropoxycellulose, hydroxyethylcellulose, carboxymethylcellulose, and polyvinyl alcohol. It is particularly preferred to use methylcellulose and hydroxypropoxycellulose in combination. The binder may be one type or two or more types may be used in combination.
[0044] Examples of the plasticizer include polyoxyalkylene alkyl ethers, polycarboxylic acid-based polymers, and alkyl phosphates.
[0045] As the dispersant, a surfactant such as polyoxyalkylene alkyl ether, ethylene glycol, dextrin, fatty acid soap, or polyol may be used. The dispersant may be used alone or in combination of two or more.
[0046] The molding method is not particularly limited, and known methods such as extrusion molding can be used. In extrusion molding, a molded body of a desired shape can be obtained by selecting a mold and a fixture of an appropriate shape. For example, in the case of obtaining a honeycomb-shaped molded body, the shape and density of the cells, the number, length and thickness of the partition walls, the shape and thickness of the outer peripheral wall and the inner peripheral wall, etc. can be controlled by selecting a mold and a fixture of an appropriate shape.
[0047] The shape of the molded body obtained by the molding process is not particularly limited, but preferably has the following honeycomb shape or hollow honeycomb shape. The honeycomb shape is a shape having an outer peripheral wall and multiple partitions arranged on the inner side of the outer peripheral wall and dividing multiple cells extending from the first end face to the second end face; the hollow honeycomb shape is a shape having an inner peripheral wall, an outer peripheral wall, and multiple partitions arranged between the inner peripheral wall and the outer peripheral wall and dividing multiple cells extending from the first end face to the second end face. By setting it to such a shape, for example, when used in a heat exchanger, its performance (such as heat recovery) can be improved.
[0048] Here, a cross-sectional view of a honeycomb-shaped molded body (honeycomb molded body) perpendicular to the cell extending direction is shown. Figure 2 A cross-sectional view of a molded body having a hollow honeycomb shape (hollow honeycomb molded body) perpendicular to the cell extension direction is shown in FIG. Figure 3 .
[0049] like Figure 2 As shown, the honeycomb molded body 100 includes an outer peripheral wall 110 and a plurality of partition walls 130 disposed inside the outer peripheral wall 110 and defining a plurality of cells 120 extending from a first end surface to a second end surface. Figure 3As shown, the hollow honeycomb formed body 200 includes an inner peripheral wall 140 , an outer peripheral wall 110 , and a plurality of partition walls 130 disposed between the inner peripheral wall 140 and the outer peripheral wall 110 and defining a plurality of cells 120 extending from a first end surface to a second end surface.
[0050] The shape (outer shape) of the honeycomb formed body 100 and the hollow honeycomb formed body 200 is not particularly limited, and may be, for example, a cylinder, an elliptical cylinder, a quadrangular prism or other polygonal prisms, etc. That is, the outer shape of the honeycomb formed body 100 and the hollow honeycomb formed body 200 in the cross section perpendicular to the extending direction of the cells 120 may be set to a circular shape, an elliptical shape, a quadrangular shape or other polygonal shape, etc. In addition, the hollow portion of the hollow honeycomb formed body 200 may be the same as or different from the outer shape of the hollow honeycomb formed body 200, and may be the various shapes mentioned above.
[0051] The shape of the cells 120 in a cross section perpendicular to the extending direction of the cells 120 is not limited to the shape shown in the figure, and may be a circle, an ellipse, a triangle or other polygonal shape.
[0052] The honeycomb formed body 100 and the hollow honeycomb formed body 200 preferably have structures satisfying the following characteristics after the firing and impregnation steps: The honeycomb formed body 100 and the hollow honeycomb formed body 200 after the firing and impregnation steps are referred to as honeycomb structures.
[0053] The cell density (i.e., the number of cells 120 per unit area) in a cross section of the honeycomb structure perpendicular to the extending direction of the cells 120 may be appropriately adjusted according to the application, and is preferably 4 to 320 cells / cm 2 In the cross section perpendicular to the extending direction of the cell 120, the cell density is set to 4 cells / cm 2 As described above, the strength of the partition walls 130 and the strength and effective GSA (geometric surface area) of the honeycomb structure itself can be sufficiently ensured. 2 Thereby, it is possible to prevent an increase in pressure loss when the fluid flows.
[0054] The thickness of the partition wall 130 of the honeycomb structure can be appropriately designed according to the purpose, preferably 50 μm to 2 mm, more preferably 60 μm to 600 μm. If the thickness of the partition wall 130 is set to 50 μm or more, the mechanical strength is improved, and the damage caused by impact and thermal stress can be suppressed. On the other hand, if the thickness of the partition wall 130 is set to 2 mm or less, the proportion of the cell volume in the honeycomb structure becomes larger, thereby reducing the pressure loss of the fluid and improving the heat exchange rate.
[0055] The thickness of the outer peripheral wall 110 and the inner peripheral wall 140 (when present) of the honeycomb structure can also be appropriately designed according to the purpose, but when used for heat exchange, it is preferably more than 0.3 mm and less than 10 mm, more preferably 0.5 mm to 5 mm, and further preferably 1 mm to 3 mm. In addition, when used for heat storage purposes, the thickness of the outer peripheral wall 110 can also be set to 10 mm or more to increase the heat capacity of the outer peripheral wall 110.
[0056] <Firing and impregnation process>
[0057] The firing and impregnation step is a step of firing the molded body and impregnating the molded body with metal Si.
[0058] The conditions of the calcining and impregnation steps are not particularly limited and can be carried out according to a known method. In addition, the calcining and impregnation steps can be carried out in one step, or can be carried out in separate steps. Specifically, the calcining step and the impregnation step can also be carried out as different steps.
[0059] The firing and impregnation steps are preferably performed by firing the molded body in a state where the molded body is in contact with the metal Si. By firing in such a state, the molten metal Si enters the gaps between the ceramic particles constituting the molded body by capillary phenomenon, thereby enabling the metal Si to be impregnated. In addition, according to such a method, firing and impregnation can be performed in one step, thereby reducing the manufacturing cost.
[0060] The position where the metal Si is brought into contact with the molded body is not particularly limited, and it is preferred that the metal Si is arranged and brought into contact with the upper surface of the molded body. For example, when the honeycomb molded body 100 and the hollow honeycomb molded body 200 are used as the molded body, the position where the metal Si is brought into contact with the molded body may be any one of the end face (the first end face or the second end face), the outer peripheral wall 110, and the inner peripheral wall 140 (when present). When the extending direction of the cells 120 is set to the vertical direction, it is preferred that the metal Si is arranged and brought into contact with the end face (the first end face or the second end face) located above the honeycomb molded body 100 and the hollow honeycomb molded body 200, thereby making it easy to impregnate the metal Si by gravity.
[0061] The firing is preferably performed in an inert gas atmosphere or in a vacuum at a temperature of 1400 to 1600° C. By firing under such conditions, metal Si can be easily impregnated. In addition, insufficient sintering due to oxidation can be suppressed, and oxides contained in the molding material can be reduced.
[0062] Examples of the inert gas atmosphere include a nitrogen atmosphere, an inert gas atmosphere such as an argon atmosphere, and a mixed gas atmosphere thereof.
[0063] From the viewpoint of stably ensuring the above-mentioned effects, the calcination temperature is preferably 1450 to 1550° C. The calcination time is not particularly limited, but is typically 0.25 to 5 hours.
[0064] In addition, the firing furnace used for firing is not particularly limited, and an electric furnace, a gas furnace, etc. can be used.
[0065] <Other Process>
[0066] Between the molding step and the firing and impregnation step, the molded body may be subjected to at least one of a drying treatment and a degreasing treatment. In addition, after the firing and impregnation step, surface processing such as grinding may be performed.
[0067] The drying process is not particularly limited, and a known method can be used. For example, the drying process can be carried out using a microwave dryer, a hot air dryer, a dielectric dryer, a reduced pressure dryer, a vacuum dryer, a freeze dryer, or the like.
[0068] The degreasing treatment is a process for burning and removing components such as a binder. The conditions of the degreasing treatment are not particularly limited as long as the binder can be burned, and can be appropriately set according to the type of the binder. For example, the degreasing treatment can be performed by heating the molded body at 300 to 600° C. for 1 to 10 hours.
[0069] (2) Ceramic body
[0070] The ceramic body according to the embodiment of the present invention is obtained by the above-mentioned method for producing a ceramic body. The ceramic body includes a SiC skeleton portion and a metal Si impregnation portion.
[0071] The SiC skeleton contains SiC particles with a particle size of 15 to 50 μm and SiC particles with a particle size of 2 to 8 μm in a volume ratio of 3:7 to 7:3. By setting the SiC skeleton to contain two types of SiC particles with a predetermined particle size in the above volume ratio, the proportion of SiC particles in the ceramic body can be increased, thereby improving the thermal conductivity of the ceramic body.
[0072] Here, the volume ratio of SiC particles with a particle size of 15 to 50 μm to SiC particles with a particle size of 2 to 8 μm in the ceramic body can be obtained by SEM observation of the cross section of the ceramic body. Specifically, in the SEM image of the cross section of the ceramic body, SiC particles with a particle size of 15 to 50 μm and SiC particles with a particle size of 2 to 8 μm are distinguished. At this time, the particle size of the SiC particles is the equivalent circle diameter. Moreover, the ratio of the total area of SiC particles with a particle size of 15 to 50 μm to the total area of SiC particles with a particle size of 2 to 8 μm is used as the volume ratio of SiC particles with a particle size of 15 to 50 μm to SiC particles with a particle size of 2 to 8 μm in the ceramic body.
[0073] The metal Si impregnation part is formed in at least a part of the voids of the SiC skeleton part. By forming the metal Si impregnation part, the ceramic body can be made dense, and the thermal conductivity and strength can be improved.
[0074] The thermal conductivity of the ceramic body is not particularly limited, but is preferably 140 W / mK or more, more preferably 150 W / mK or more at 25°C. When the ceramic body is used in a heat exchanger, the heat recovery of the heat exchanger can be improved by setting the thermal conductivity of the ceramic body to the above range. It should be noted that the value of the thermal conductivity refers to the value measured by the laser flash method (JIS R1611: 1997).
[0075] Other features such as the material constituting the ceramic body and its shape are as described in the above-mentioned method for producing the ceramic body, and the description thereof is omitted.
[0076] Example
[0077] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples at all.
[0078] (Example 1 to Example 4)
[0079] Three types of SiC powders having average particle diameters D50 of 35 μm, 25 μm, and 5 μm were prepared.
[0080] Next, two or three of these SiC powders were mixed in the mass ratio shown in Table 1, and 28 parts by mass of water and 7 parts by mass of methyl cellulose were further added to 100 parts by mass of the total amount of the SiC powder to obtain a molding material. The molding material was extruded to obtain a honeycomb-shaped molding. The size of the honeycomb molding was adjusted so that after firing and impregnation, a honeycomb structure of the following shape was obtained.
[0081] Shape of the honeycomb structure in a cross section perpendicular to the cell extension direction: circular
[0082] The shape of the cell in the cross section perpendicular to the cell extension direction: quadrilateral
[0083] Length of hole extension direction: 100mm
[0084] The outer diameter of the honeycomb structure in the cross section perpendicular to the cell extension direction: 100 mm
[0085] Cell density: 14 cells / cm 2
[0086] Thickness of the wall: 0.3mm
[0087] Thickness of outer wall: 1.5mm
[0088] Next, the honeycomb formed body was arranged so that the cell extending direction was the vertical direction, metal Si was arranged on the upper end surface, and then fired at 1500° C. in a vacuum to obtain a honeycomb structure (ceramic body).
[0089] (Comparative Example 1 and Comparative Example 2)
[0090] A honeycomb structure (ceramic body) was obtained in the same manner as in the above-mentioned Example except that SiC powder having an average particle size D50 of 35 μm or SiC powder having an average particle size D50 of 5 μm was used alone.
[0091] The thermal conductivity of the honeycomb structure obtained above was measured at 25° C. using a laser flash method (JIS R 1611: 1997). In the evaluation of the thermal conductivity, a thermal conductivity of 150 W / mK or more was indicated as ◎, a thermal conductivity of 140 W / mK or more and less than 150 W / mK was indicated as 0, and a thermal conductivity of less than 140 W / mK was indicated as ×. The results are shown in Table 1.
[0092] [Table 1]
[0093]
[0094] As shown in Table 1, the honeycomb structures (ceramic bodies) of Examples 1 to 4, which are made using SiC powder with an average particle size D50 of 15 to 50 μm and SiC powder with an average particle size D50 of 2 to 8 μm in a mass ratio of 3:7 to 7:3, have higher thermal conductivity than the honeycomb structures (ceramic bodies) of Comparative Examples 1 and 2, which are made using a single SiC powder.
[0095] As is apparent from the above results, according to the present invention, a ceramic body having high thermal conductivity and composed of Si-impregnated SiC and a method for producing the same can be provided.
Claims
1. A method for manufacturing a ceramic body, comprising: a molding step of molding a molding material containing SiC powder having an average particle size D50 of 15 to 50 μm and SiC powder having an average particle size D50 of 2 to 8 μm in a mass ratio of 3:7 to 7:3 to obtain a molded body, and The calcination and impregnation step is to perform calcination of the molded body and impregnation of metal Si.
2. The method for producing a ceramic body according to claim 1, wherein: The calcination and impregnation steps are performed by calcining the molded body in a state where the molded body is in contact with metal Si.
3. The method for manufacturing a ceramic body according to claim 2, wherein: The calcination is performed at a temperature of 1400 to 1600° C. in an inert gas atmosphere or in a vacuum.
4. The method for producing a ceramic body according to any one of claims 1 to 3, wherein: The ceramic raw material contained in the molding material is only the SiC powder.
5. The method for producing a ceramic body according to any one of claims 1 to 3, wherein: Between the molding step and the firing and impregnation step, the molded body is subjected to at least one of a drying treatment and a degreasing treatment.
6. The method for producing a ceramic body according to any one of claims 1 to 3, wherein: The molded body has a honeycomb shape or a hollow honeycomb shape, The honeycomb shape has an outer peripheral wall and a plurality of partition walls disposed inside the outer peripheral wall and defining a plurality of cells extending from a first end surface to a second end surface; The hollow honeycomb has an inner peripheral wall, an outer peripheral wall, and a plurality of partition walls disposed between the inner peripheral wall and the outer peripheral wall and defining a plurality of cells extending from a first end surface to a second end surface.
7. A ceramic body comprising: A SiC skeleton portion containing SiC particles having a particle size of 15 to 50 μm and SiC particles having a particle size of 2 to 8 μm at a volume ratio of 3:7 to 7:3; and The metal Si impregnation portion is formed in at least a portion of the voids in the SiC skeleton portion.
Citation Information
Patent Citations
Si-siC particles fired body and production method thereof
CN101172861A
Honeycomb structure production method
CN109311771A
Silicon-impregnated silicon carbide-based material for heat treatment of semiconductor, and its production
JP2000103677A
Heat exchange member and ceramics structure
JP2015042934A