Aluminum nitride ceramic material for HTCC and preparation method thereof

Through the combined ingredients and process steps of modified aluminum nitride powder and refined sintering aid, aluminum nitride ceramic materials for HTCC with high thermal conductivity and high flexural strength are prepared, solving the thermal conductivity problems of existing aluminum nitride ceramic materials. It solves the problems of low efficiency and insufficient bending strength and meets the complex needs of microelectronic devices.

CN118724596AActive Publication Date: 2024-10-01GUIYANG SUNLORD SCHINDLER ELECTRONICS CO LTD

Patent Information

Application Number
CN202411090807.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-01
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing aluminum nitride ceramic materials have low thermal conductivity and insufficient flexural strength, and cannot meet the complex requirements for thermal conductivity and strength of microelectronic devices.

Method used

Aluminum nitride ceramic materials for HTCC are prepared using a combination of modified aluminum nitride powder and refined sintering aids, through surface modification, sand grinding, ball milling, degassing, tape casting, debinding and sintering. Improve its thermal conductivity and flexural strength.

Benefits of technology

Aluminum nitride ceramic materials with high thermal conductivity and high flexural strength have been realized. The thermal conductivity reaches more than 200W/(m·K) and the flexural strength exceeds 400MPa, which meets the requirements of microelectronic devices and is improved by improving the microstructure. Comprehensive properties of ceramics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724596A_ABST
    Figure CN118724596A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum nitride ceramic material for HTCC and a preparation method thereof, and belongs to the technical field of aluminum nitride ceramic materials for HTCC, the aluminum nitride ceramic material is prepared from the following ingredients in parts by mass: 45-55 parts of modified aluminum nitride powder, 2-3 parts of a sanding and sintering aid, 30-40 parts of a solvent, 1.5-5 parts of a dispersing agent, 0.5-1 part of a binder and 7-10 parts of a plasticizer, and the aluminum nitride ceramic material is prepared from the ingredients. According to the aluminum nitride ceramic material for the HTCC, the modified aluminum oxide powder is matched with other components, the aluminum nitride ceramic material for the HTCC is prepared according to the proportion, the aluminum nitride ceramic with high heat conductivity and high bending strength is achieved, the problem that existing aluminum nitride ceramic is low in heat conductivity is solved, the heat conductivity coefficient reaches 200 W / (mK) or above, the bending strength is 400 Mpa or above, and the use requirements of devices can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum nitride ceramic materials for HTCC, and specifically relates to an aluminum nitride ceramic material for HTCC, and also relates to a preparation method of the aluminum nitride ceramic material for HTCC. Background Art

[0002] With the rapid development of microelectronics technology, devices are required to develop in the direction of large capacity, high density, high speed and high power output. More and more complex devices have put forward higher and higher requirements on the thermal conductivity and strength of packaging materials. Aluminum nitride is a new type of ceramic material with excellent comprehensive performance. It has high thermal conductivity, relatively low dielectric constant and dielectric loss, and a thermal expansion coefficient that matches chip materials such as silicon and gallium arsenide (the thermal expansion coefficient is about 3.5×10 -6 K -1 ~4.8×10 -6 K -1 ), non-toxic, insulating and other excellent properties, it is considered to be the first choice material for the ideal material of the new generation of electronic device packaging, and has been widely used in electronics, automobiles, aerospace and other fields.

[0003] Aluminum nitride ceramics are sintered from aluminum nitride powder. The main factors affecting the performance of aluminum nitride ceramics include the performance of aluminum nitride powder, the type of sintering aid, and the sintering process. The performance of aluminum nitride powder is the key to determining the preparation process and quality of aluminum nitride ceramics. Theoretically, the thermal conductivity of aluminum nitride is 320W / (m·K), but aluminum nitride powder is easily hydrolyzed in the air, and oxygen impurities diffuse into the aluminum nitride lattice during the sintering process, resulting in a decrease in the thermal conductivity of aluminum nitride ceramics. The actual thermal conductivity of aluminum nitride ceramics produced is generally below 180W / (m·K). The flexural strength of aluminum nitride ceramics is only between 300 and 390MPa, which cannot meet the needs of the microelectronics packaging industry and limits the application range of aluminum nitride ceramics. At present, it is of great significance to develop new methods to prepare aluminum nitride ceramics with high thermal conductivity and high flexural strength. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an aluminum nitride ceramic material for HTCC and a preparation method thereof, so as to obtain aluminum nitride ceramics with high thermal conductivity and high bending strength, and solve the problem of low thermal conductivity of existing aluminum nitride ceramics.

[0005] The technical solution adopted by the present invention is: an aluminum nitride ceramic material for HTCC, comprising the following ingredients in mass ratio:

[0006] Aluminum nitride ceramic material is prepared by mixing 45-55 of modified aluminum nitride powder, 2-3 of sand grinding sintering aid, 30-40 of solvent, 1.5-5 of dispersant, 1-3 of binder and 5-7 of plasticizer.

[0007] Furthermore, the method for preparing the aluminum nitride ceramic material for HTCC comprises the following steps:

[0008] Step 1: Modification and sand grinding: Surface modification of aluminum nitride powder and sand grinding of sintering aid;

[0009] Step 2, primary and secondary ball milling: adding the modified aluminum nitride powder, the sintering aid after sand milling, the solvent and the dispersant together into a ball mill for primary ball milling, and adding the binder and the plasticizer for secondary ball milling after the primary ball milling;

[0010] Step 3, degassing: after the second ball milling, the ball milled slurry is vacuum degassed by a vacuum degassing machine to obtain a ceramic slurry;

[0011] Step 4, tape casting: tape casting the ceramic slurry and drying it to obtain a ceramic green body;

[0012] Step 5: Slicing: cutting the ceramic green body into green sheets;

[0013] Step 6: Debinding: Put the blank into the debinding furnace for debinding;

[0014] Step 7: Sintering: Aluminum nitride ceramics with high thermal conductivity and high bending strength are obtained by high-temperature sintering in a vacuum furnace.

[0015] Furthermore, the surface modification treatment formula is as follows: the mass ratio of aluminum nitride powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0016] Furthermore, the surface modification treatment method is as follows: aluminum nitride powder, citric acid and silane coupling agent are added to a set amount of anhydrous ethanol to obtain an aluminum nitride mixed slurry, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball milling speed is 300 to 600 r / min, and the dispersion time is 8 to 12 hours. The uniform aluminum nitride mixed slurry after ball milling is placed in an oven for drying at a drying temperature of 80 to 100°C to prepare modified aluminum nitride powder.

[0017] Furthermore, the sand grinding and refining method of the above-mentioned sintering aid is: yttrium oxide, calcium fluoride, magnesium fluoride, and lanthanum oxide are selected as sintering aids, and the sintering aids are sand ground in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1.2 μm, the sand grinding temperature is 20 to 35°C, and then placed in an oven for drying at a drying temperature of 80 to 100°C to obtain a sintering aid powder of 0.4 to 1.2 μm, wherein the mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0018] Furthermore, the above-mentioned primary ball milling and secondary ball milling methods are: adding the modified aluminum nitride powder, the sand-milled sintering aid, the solvent, and the dispersant into a ball mill, ball milling for 16 to 24 hours, and then adding a binder and a plasticizer to continue ball milling for 16 to 24 hours (the purpose of the primary grinding is to evenly disperse the aluminum nitride and the sintering aid; the secondary ball milling is to add a binder to make the slurry cohesive and the green body after casting has suitable strength), the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0019] Furthermore, the cut blank is 30mm*50mm*1.5mm.

[0020] Furthermore, the above debinding method is: placing the green sheet into an atmosphere debinding furnace for debinding, and the debinding temperature is 250-600°C.

[0021] Furthermore, the sintering method is as follows: the green sheet after debinding is sintered at a sintering temperature of 1750-1900° C., and after sintering, it is cooled to room temperature to obtain an aluminum nitride ceramic sheet.

[0022] Beneficial effects of the present invention: Compared with the prior art, the effects of the present invention are as follows:

[0023] (1) Aluminum nitride ceramic materials for HTCC are prepared by using modified alumina powder and other ingredients in a proportion to achieve high thermal conductivity and high bending strength aluminum nitride ceramics, solving the problem of low thermal conductivity of existing aluminum nitride ceramics. The thermal conductivity reaches more than 200W / (m·K) and the bending strength reaches more than 400Mpa, which can meet the use requirements of the device, that is, it can meet the minimum thermal conductivity of 170W / (m·K) and the minimum bending strength of 350Mpa required for aluminum nitride ceramic materials for HTCC;

[0024] (2) Pre-treating the aluminum nitride powder and the sintering aid to prevent the aluminum nitride green tape from being hydrolyzed during the subsequent storage and pre-curing process, forming an aluminum oxide film on the surface of the aluminum nitride, eliminating the reaction between the aluminum oxide film and yttrium oxide to form the yttrium aluminate phase, greatly reducing the content of the yttrium aluminate phase between the aluminum nitride grains, reducing the mismatch of the thermal expansion coefficients of the aluminum nitride and the yttrium aluminate phase, and improving the strength of the ceramic;

[0025] (3) It can be seen from the electron micrograph that the aluminum nitride ceramics obtained by the modified aluminum nitride powder and the refined sintering aid method have no pores in the cross-section electron micrograph and the ceramics have better sintering density. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the electron microscope image of comparative example 1;

[0027] Figure 2 is an electron microscope image of Example 1;

[0028] Figure 3 It is a preparation flow chart. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0030] Embodiment: An aluminum nitride ceramic material for HTCC includes the following ingredients in mass ratio:

[0031] 45-55 of modified aluminum nitride powder, 2-3 of sand grinding sintering aid, 30-40 of solvent, 1.5-5 of dispersant, 0.5-1 of binder and 7-10 of plasticizer are used to prepare aluminum nitride ceramic material. The preparation method of the aluminum nitride ceramic material for HTCC comprises the following steps:

[0032] Step 1. Aluminum nitride surface modification

[0033] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0034] Step 2. Sanding of sintering aid

[0035] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1.2 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0036] Step 3. Ball milling

[0037] Add modified aluminum nitride powder, refined sintering aid, solvent and dispersant into a ball mill, and ball mill for 16 to 24 hours. Then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0038] Step 4. Degassing

[0039] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0040] Step 5. Tape casting

[0041] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0042] Step 6. Cutting

[0043] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0044] Step 7. Debonding

[0045] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0046] Step 8. Sintering

[0047] The green sheet after debinding is sintered at a temperature of 1750-1900° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0048] Embodiment 1: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0049] 1. Surface modification of aluminum nitride

[0050] Add AlN powder, citric acid and silane coupling agent into an appropriate amount of anhydrous ethanol, and use a ball mill to disperse the aluminum nitride mixed slurry evenly. The ball mill speed is 300-600r / min, and the dispersion time is 8-

[0051] The uniform mixed slurry is dried in an oven at a drying temperature of 80-100° C. to prepare modified aluminum nitride powder, wherein the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0052] 2. Sand grinding of sintering aid

[0053] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 45%, the mass fraction of calcium fluoride is 30%, the mass fraction of magnesium fluoride is 20%, and the mass fraction of lanthanum oxide is 5%.

[0054] 3. Ball milling

[0055] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer is 55:3:40:5:3:7, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0056] 4.Degassing

[0057] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0058] 5. Casting

[0059] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0060] 6. Cutting

[0061] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0062] 7. Glue removal

[0063] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0064] 8. Sintering

[0065] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0066] Embodiment 2: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0067] 1. Surface modification of aluminum nitride

[0068] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0069] 2. Sand grinding of sintering aid

[0070] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0071] 3. Ball milling

[0072] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 55:2.5:35:3:2:6, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0073] 4.Degassing

[0074] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0075] 5. Casting

[0076] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0077] 6. Cutting

[0078] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0079] 7. Glue removal

[0080] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0081] 8. Sintering

[0082] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0083] Embodiment 3: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0084] 1. Surface modification of aluminum nitride

[0085] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0086] 2. Sand grinding of sintering aid

[0087] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0088] 3. Ball milling

[0089] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 55:2:30:1.5:1:5, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0090] 4.Degassing

[0091] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0092] 5. Casting

[0093] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0094] 6. Cutting

[0095] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0096] 7. Glue removal

[0097] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0098] 8. Sintering

[0099] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0100] Embodiment 4: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0101] 1. Surface modification of aluminum nitride

[0102] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0103] 2. Sand grinding of sintering aid

[0104] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0105] 3. Ball milling

[0106] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 50:3:40:5:3:7, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0107] 4.Degassing

[0108] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0109] 5. Casting

[0110] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0111] 6. Cutting

[0112] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0113] 7. Glue removal

[0114] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0115] 8. Sintering

[0116] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0117] Embodiment 5: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0118] 1. Surface modification of aluminum nitride

[0119] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0120] 2. Sand grinding of sintering aid

[0121] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0122] 3. Ball milling

[0123] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 50:2.5:35:3:2:6, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0124] 4.Degassing

[0125] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0126] 5. Casting

[0127] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0128] 6. Cutting

[0129] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0130] 7. Glue removal

[0131] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0132] 8. Sintering

[0133] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0134] Embodiment 6: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0135] 1. Surface modification of aluminum nitride

[0136] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0137] 2. Sand grinding of sintering aid

[0138] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0139] 3. Ball milling

[0140] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 50:2:30:1.5:1:5, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0141] 4.Degassing

[0142] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0143] 5. Casting

[0144] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0145] 6. Cutting

[0146] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0147] 7. Glue removal

[0148] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0149] 8. Sintering

[0150] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0151] Embodiment 7: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0152] 1. Surface modification of aluminum nitride

[0153] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0154] 2. Sand grinding of sintering aid

[0155] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0156] 3. Ball milling

[0157] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 45:3:40:5:3:7, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0158] 4.Degassing

[0159] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0160] 5. Casting

[0161] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0162] 6. Cutting

[0163] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0164] 7. Glue removal

[0165] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0166] 8. Sintering

[0167] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0168] Embodiment 8: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0169] 1. Surface modification of aluminum nitride

[0170] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0171] 2. Sand grinding of sintering aid

[0172] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0173] 3. Ball milling

[0174] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 45:2.5:35:3:2:6, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0175] 4.Degassing

[0176] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0177] 5. Casting

[0178] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0179] 6. Cutting

[0180] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0181] 7. Glue removal

[0182] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0183] 8. Sintering

[0184] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0185] Embodiment 9: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0186] 1. Surface modification of aluminum nitride

[0187] AlN powder, citric acid and silane coupling agent are added to an appropriate amount of anhydrous ethanol, and the aluminum nitride mixed slurry is evenly dispersed using a ball mill, the ball mill speed is 300-600r / min, and the dispersion time is 8-12h. The obtained uniform mixed slurry is dried in an oven at a drying temperature of 80-100°C to prepare modified aluminum nitride powder, and the mass ratio of AlN powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

[0188] 2. Sand grinding of sintering aid

[0189] Yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand-milled in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1 μm, the sand-milling temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying, the drying temperature is 80 to 100° C., and a finer sintering aid powder is obtained. The mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 25-35%, the mass fraction of magnesium fluoride is 15-25%, and the mass fraction of lanthanum oxide is 5-10%.

[0190] 3. Ball milling

[0191] Add modified aluminum nitride powder, refined sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The mass ratio of modified aluminum nitride powder, sand milling sintering aid, solvent, dispersant, binder, and plasticizer used is 45:2:30:1.5:1:5, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0192] 4.Degassing

[0193] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0194] 5. Casting

[0195] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0196] 6. Cutting

[0197] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0198] 7. Glue removal

[0199] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0200] 8. Sintering

[0201] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0202] Comparative Example 1: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0203] 1. Ball milling

[0204] Aluminum nitride powder, sintering aid, solvent, and dispersant are added to a ball mill, and ball milling is performed for 16 to 24 hours. Then, a binder and a plasticizer are added and ball milling is continued for 16 to 24 hours. The mass ratio of aluminum nitride powder, sintering aid, solvent, dispersant, binder, and plasticizer used is 55:3:40:5:3:7. The sintering aid is yttrium oxide, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0205] 2.Degassing

[0206] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0207] 3. Casting

[0208] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0209] 4. Cutting

[0210] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0211] 5. Glue removal

[0212] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0213] 6. Sintering

[0214] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0215] Comparative Example 2: A method for preparing an aluminum nitride ceramic material for HTCC, comprising the following steps:

[0216] 1. Ball milling

[0217] Aluminum nitride powder, sintering aid, solvent, and dispersant are added to a ball mill, ball milled for 16 to 24 hours, and then a binder and a plasticizer are added and ball milled for 16 to 24 hours. The mass ratio of aluminum nitride powder, sintering aid, solvent, dispersant, binder, and plasticizer used is 55:3:40:5:3:7, the mass fraction of yttrium oxide in the sintering aid is 45%, the mass fraction of calcium fluoride is 30%, the mass fraction of magnesium fluoride is 20%, and the mass fraction of lanthanum oxide is 5%, the solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0218] 2.Degassing

[0219] The ball-milled material is sent to a degassing machine for degassing treatment to obtain ceramic slurry.

[0220] 3. Casting

[0221] The defoamed ceramic slurry is tape-casted by a tape casting machine to obtain a green tape.

[0222] 4. Cutting

[0223] The green tape is cut into green sheets of 30 mm*50 mm*1.5 mm in size.

[0224] 5. Glue removal

[0225] The blank is placed in an atmosphere debinding furnace for debinding at a debinding temperature of 250-600°C.

[0226] 6. Sintering

[0227] The green sheet after debinding is sintered at a temperature of 1850° C. and cooled to room temperature after sintering to obtain an aluminum nitride ceramic sheet.

[0228] A high thermal conductivity and high bending strength aluminum nitride ceramic material for HTCC, whose thermal conductivity is greater than 200W / (m·K) and bending strength is greater than 400MPa. The aluminum nitride ceramic prepared by the present invention has excellent thermal and mechanical properties, which is mainly attributed to the refinement of aluminum nitride modification and sintering aid, which promotes the densification of aluminum nitride ceramics, improves the microstructure, grain size, and composition and distribution of the crystalline phase of aluminum nitride ceramics, thereby achieving the improvement of the comprehensive performance of aluminum nitride ceramics. Table 1 shows the density, thermal conductivity and bending strength of each embodiment and comparative example. It can be seen that embodiments 1, 2, and 3 have better and more excellent performance than comparative examples 1 and 2. Figure 1 , Figure 2 These are the electron microscopy results of comparative example 1 and embodiment 1, respectively. It can be seen that in the aluminum nitride ceramics obtained by the modified aluminum nitride powder and the refined sintering aid method, there are no pores in the cross-section electron microscopy, and the ceramics have reached the level of sintering density.

[0229] Table 1 Thermal conductivity and flexural strength

[0230] <![CDATA[Density (g / cm 3 )]]> Thermal conductivity (W / (m·K)) Flexural strength(MPa) Embodiment 1 3.36 206 420 Embodiment 2 3.35 220 432 Embodiment 3 3.35 210 450 Embodiment 4 3.35 203 441 Embodiment 5 3.36 208 428 Embodiment 6 3.37 214 409 Embodiment 7 3.35 223 460 Embodiment 8 3.36 205 430 Embodiment 9 3.36 216 421 Comparative Example 1 3.29 170 380 Comparative Example 2 3.32 185 401

[0231] 2. The formula of ceramic material is as follows: the mass ratio of modified aluminum nitride powder, sand grinding sintering aid, solvent, dispersant, binder and plasticizer is 45-55:2-3:30-40:1.5-5:1-3:5-7.

[0232] Among them, the mass ratio of the aluminum nitride ceramic in Example 1 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 55:1.35:0.9:0.6:0.15; the mass ratio of the aluminum nitride ceramic in Example 2 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 55:1.125:0.75:0.5:0.125; the mass ratio of the aluminum nitride ceramic in Example 3 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride : lanthanum oxide = 55:0.9:0.6:0.4:0.1; the mass ratio of the aluminum nitride ceramic of Example 4 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.35:0.9:0.6:0.15; the mass ratio of the aluminum nitride ceramic of Example 5 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.125:0.75:0.5:0.125; the mass ratio of the aluminum nitride ceramic of Example 6 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.125:0.75:0.5:0.125; the mass ratio of the aluminum nitride ceramic of Example 7 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.125:0.75:0.5:0.125; the mass ratio of the aluminum nitride ceramic of Example 8 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.125:0.75:0.5:0.125 The mass ratio of the aluminum nitride ceramics is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.35:0.9:0.6:0.15; the mass ratio of the aluminum nitride ceramics in Example 7 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 45:1.35:0.9:0.6:0.15; the mass ratio of the aluminum nitride ceramics in Example 8 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 45:1.35:0. 9:0.6:0.15; the mass ratio of the aluminum nitride ceramic of Example 9 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 45:0.9:0.6:0.4:0.1; the mass ratio of the aluminum nitride ceramic of Comparative Example 1 is aluminum nitride: yttrium oxide = 50:3; the mass ratio of the aluminum nitride ceramic of Comparative Example 2 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.35:0.9:0.6:0.15.

[0233] The present invention has the following advantages:

[0234] 1. Pre-treat aluminum nitride powder and sintering aids to prevent the cast aluminum nitride green tape from hydrolyzing during subsequent storage and pre-curing processes, form an aluminum oxide film on the surface of aluminum nitride, eliminate the reaction between the aluminum oxide film and yttrium oxide to form yttrium aluminate phase, greatly reduce the content of yttrium aluminate phase between aluminum nitride grains, reduce the mismatch of thermal expansion coefficients between aluminum nitride and yttrium aluminate phase, and improve the strength of ceramics;

[0235] 2. In the ceramic material formula, the mass ratio of the aluminum nitride ceramic in Example 1 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 55:1.35:0.9:0.6:0.15; the mass ratio of the aluminum nitride ceramic in Example 2 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 55:1.125:0.75:0.5:0.125; the mass ratio of the aluminum nitride ceramic in Example 3 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 55:1.125:0.75:0.5:0.125. Calcium: magnesium fluoride: lanthanum oxide = 55: 0.9: 0.6: 0.4: 0.1; the mass ratio of the aluminum nitride ceramic of Example 4 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50: 1.35: 0.9: 0.6: 0.15; the mass ratio of the aluminum nitride ceramic of Example 5 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50: 1.125: 0.75: 0.5: 0.125; the mass ratio of the aluminum nitride ceramic of Example 6 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50: 1.125: 0.75: 0.5: 0.125; The mass ratio of aluminum nitride ceramic is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.35:0.9:0.6:0.15; the mass ratio of aluminum nitride ceramic in Example 7 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 45:1.35:0.9:0.6:0.15; the mass ratio of aluminum nitride ceramic in Example 8 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 45:1.35: 0.9:0.6:0.15; the mass ratio of the aluminum nitride ceramic of Example 9 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 45:0.9:0.6:0.4:0.1; the mass ratio of the aluminum nitride ceramic of Comparative Example 1 is aluminum nitride: yttrium oxide = 50:3; the mass ratio of the aluminum nitride ceramic of Comparative Example 2 is aluminum nitride: yttrium oxide: calcium fluoride: magnesium fluoride: lanthanum oxide = 50:1.35:0.9:0.6:0.15.

[0236] 3. From the electron microscopy results of Comparative Example 1 and Example 1, it can be seen that the aluminum nitride ceramics obtained by using the modified aluminum nitride powder and the refined sintering aid method have no pores in the cross-section electron microscopy and the ceramics have better sintering density.

[0237] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. An aluminum nitride ceramic material for HTCC, characterized in that: The invention comprises the following ingredients in mass ratio: Aluminum nitride ceramic material is prepared by mixing 45-55 of modified aluminum nitride powder, 2-3 of sand grinding sintering aid, 30-40 of solvent, 1.5-5 of dispersant, 1-3 of binder and 5-7 of plasticizer.

2. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The method comprises the following steps: Step 1: Modification and sand grinding: Surface modification of aluminum nitride powder and sand grinding of sintering aid; Step 2, primary and secondary ball milling: adding the modified aluminum nitride powder, the sintering aid after sand milling, the solvent and the dispersant together into a ball mill for primary ball milling, and adding the binder and the plasticizer for secondary ball milling after the primary ball milling; Step 3, degassing: after the second ball milling, the ball milled slurry is vacuum degassed by a vacuum degassing machine to obtain a ceramic slurry; Step 4, tape casting: tape casting the ceramic slurry and drying it to obtain a ceramic green body; Step 5: Slicing: cutting the ceramic green body into green sheets; Step 6: Debinding: Put the blank into the debinding furnace for debinding; Step 7: Sintering: Aluminum nitride ceramics with high thermal conductivity and high bending strength are obtained by high-temperature sintering in a vacuum furnace.

3. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The surface modification treatment formula is: the mass ratio of aluminum nitride powder, citric acid, silane coupling and anhydrous ethanol is 45-55:2-10:5-15:30-40.

4. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The surface modification treatment method is as follows: "adding aluminum nitride powder, citric acid and silane coupling agent in a mass ratio of 45%:5%:10% to 40%wt anhydrous ethanol to obtain an aluminum nitride mixed slurry, using a ball mill to evenly disperse the aluminum nitride mixed slurry, the ball milling speed is 300-600r / min, the dispersion time is 8-12h, and the uniform aluminum nitride mixed slurry after ball milling is placed in an oven for drying at a drying temperature of 80-100°C to prepare modified aluminum nitride powder.

5. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The sand grinding and refining method of the sintering aid is as follows: yttrium oxide, calcium fluoride, magnesium fluoride and lanthanum oxide are selected as sintering aids, and the sintering aids are sand ground in anhydrous ethanol to obtain a sintering aid slurry with a D50 of 0.4 to 1.2 μm, the sand grinding temperature is 20 to 35° C., and then the sintering aid slurry is placed in an oven for drying at a drying temperature of 80 to 100° C. to obtain a sintering aid powder of 0.4 to 1.2 μm, wherein the mass fraction of yttrium oxide in the sintering aid is 40-50%, the mass fraction of calcium fluoride is 20-35%, the mass fraction of magnesium fluoride is 10-25% and the mass fraction of lanthanum oxide is 5-10%.

6. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The primary and secondary ball milling methods are as follows: add modified aluminum nitride powder, sand-milled sintering aid, solvent, and dispersant into a ball mill, ball mill for 16 to 24 hours, then add a binder and a plasticizer and continue ball milling for 16 to 24 hours. The solvent is anhydrous ethanol, the dispersant is ammonium polyacrylate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

7. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The cut blank is 30mm*50mm*1.5mm.

8. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The debinding method is: putting the blank into an atmosphere debinding furnace for debinding, and the debinding temperature is 250-600℃.

9. The method for preparing an aluminum nitride ceramic material for HTCC according to claim 1, characterized in that: The sintering method is as follows: the green sheet after debinding is sintered at a temperature of 1750-1900° C., and after sintering, the green sheet is cooled to room temperature to obtain an aluminum nitride ceramic sheet.

Citation Information

Patent Citations

  • Method for preparing LED by using transparent ceramics

    CN101697367A

  • Aluminium nitride ceramic substrate, and preparation method thereof

    CN107188568A

  • Hydrolysis-resisting aluminum nitride powder and preparation method thereof

    CN107954725A

  • Fluorescent ceramic with aluminum nitride matrix and preparation method of fluorescent ceramic

    CN115947604A

  • Method for preparing aluminum nitride powder by using sand mill and aluminum nitride powder

    CN116120075A

Cited By

  • High-strength aluminum nitride ceramic substrate and preparation method thereof

    CN120329051A