Flexible wrapping synchronous reaction connection method for three-dimensional structure SiC-based ceramic connecting piece
Through the flexible graphite paper wrapping synchronous reaction connection method, the problems of large amounts of silicon powder and long heat preservation time in the traditional embedding method are solved, and the efficient preparation of large-sized, complex-shaped three-dimensional structure silicon carbide-based ceramic materials is achieved, achieving high density and excellent performance. Connectors with excellent mechanical properties, suitable for a variety of industrial applications.
Patent Information
- Application Number
- CN202410975740.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to effectively prepare large-sized, complex-shaped three-dimensional structure silicon carbide-based composite ceramic material connectors with existing technology. The traditional embedding method requires a large amount of silicon powder, has long heat preservation time and affects dimensional accuracy, and is high-cost, making it unable to meet industrial needs.
The flexible graphite paper wrapping synchronous reaction connection method is used. The graphite paper is folded and carbon fiber ropes are fixed, and silicon powder is filled for reaction infiltration to achieve the preparation of three-dimensional structure carbon fiber reinforced silicon carbide ceramic materials, reducing the amount of silicon powder and reaction time.
Successfully prepared three-dimensional structural connectors with high density, low open porosity and excellent mechanical properties, which reduced the tooling preparation cycle and cost, shortened the construction period, and is suitable for aerospace and other fields.
Smart Images

Figure CN118724602A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of SiC-based composite ceramic material connection, and in particular relates to a flexible wrapping synchronous reaction connection method for a three-dimensional SiC-based ceramic material connector. Background Art
[0002] Silicon carbide-based composite ceramic materials have been widely used in the aerospace field and other harsh service environments due to their low density, high strength, wear resistance, oxidation resistance, thermal shock resistance and corrosion resistance. At present, the demand for silicon carbide-based composite ceramic materials is developing towards large sizes and specific shapes, but silicon carbide-based composite ceramic materials have poor toughness and poor processability, and it is difficult to prepare complex-shaped parts through molding processes such as extrusion and forging. Therefore, connection technology came into being. Through connection technology, simple-shaped silicon carbide-based composite materials can be connected according to demand to obtain special parts with complex structures.
[0003] In reaction bonding, the bonding layer is mainly SiC ceramic phase. The thermal expansion coefficient of the bonding layer matches that of the parent material, and the chemical composition of the bonding layer can be adjusted within a certain range. It is an extremely attractive bonding technology for silicon carbide-based composite ceramic materials.
[0004] In the Chinese invention patent (Synchronous Reaction Connection-Preparation of Heterogeneous SiC-based Ceramic Material Connectors and Methods, 202210313101.9), the prepared phenolic resin slurry is applied to the connection surface to be connected, pressure is applied, and heating and curing is performed to prepare a pre-connector with a bonding layer, and the pre-connector is subjected to an embedding method reaction infiltration to obtain a SiC-based ceramic material connector. The embedding method uses a large amount of silicon and is only suitable for the preparation of small connectors. No attempt has been made to prepare large-sized connectors.
[0005] In the Chinese invention patent (Method for optimizing the connection joint of continuous carbon fiber reinforced SiC-based composite materials, 202311419966.4), C f The surface of the / C composite material matrix to be connected is processed with a special-shaped interface, the surface of the connection interface is treated and the connection surface is reinforced, and the resin slurry is used to connect them, and the connecting parts are wrapped by the embedding method for reactive infiltration. This method has high requirements on the processing accuracy of the matrix and high cost. The maximum sample size is 80mm×40mm×10mm, the shape is fixed, and it fails to achieve the connection of complex shapes, especially three-dimensional components, and cannot meet industrial needs.
[0006] When reactive infiltration is used to prepare three-dimensional structural ceramic material connectors, the silicon powder embedding method requires a large amount of silicon powder, a long insulation time, and excess molten silicon is easy to solidify on the surface of the component during the cooling process, affecting the dimensional accuracy. In addition, the traditional embedding method requires a customized container that can carry a large amount of melt for the development of the cavity structure, and the container scrap rate is high. Excessive melt will over-react with carbon fiber, causing its mechanical properties to drop significantly. In addition, some C / C composite materials only require local ceramic modification, which is very difficult in the traditional RMI method. Therefore, it is urgent to design a flexible tooling that fits the connector, reduce the tooling preparation cycle and cost, reduce the amount of silicon powder and reaction time of three-dimensional structural connectors, and reduce resource and energy waste. Summary of the invention
[0007] In order to realize the preparation of large-sized, complex-shaped, three-dimensional connectors, the purpose of the present invention is to provide a method for realizing a one-time synchronous reaction connection of three-dimensional structured SiC-based ceramic material connectors, by using graphite paper according to the shape of the pre-connector, the components are folded and wrapped with a certain spacing reserved to form a plurality of graphite paper toolings, and the shaped graphite paper toolings are wrapped and bundled with carbon fiber rope bundles to achieve fixation, and silicon powder is filled between the graphite paper tooling and the pre-connector to perform reaction infiltration, thereby realizing the preparation of three-dimensional structured carbon fiber reinforced silicon carbide ceramic connectors, reducing the amount of silicon powder used in the three-dimensional connectors, and achieving good density, open porosity and excellent mechanical properties.
[0008] The present invention is achieved through the following technical solutions.
[0009] According to one aspect of the present invention, a method for flexible wrapping synchronous reaction connection of a three-dimensional SiC-based ceramic connector is provided, comprising the following steps:
[0010] S1, mixing phenolic resin, ethylene glycol, benzenesulfonyl chloride, silicon carbide powder and graphite powder in a mass ratio of 1:1:0.1:(0.1-0.2):(0.1-0.15), filtering to remove bubbles, and heating in a water bath to obtain a synchronous reaction connection slurry;
[0011] S2, C f / C Polishing of the connection surface of composite material connection components;
[0012] S3, respectively C f / C composite material connecting components are connected on the connecting surface by coating with reactive connecting slurry, assembling, curing in sections, and carbonizing to obtain a pre-connected component with a three-dimensional structure;
[0013] S4, using graphite paper according to the shape of the pre-connector, the components are folded and wrapped with a certain spacing to form multiple graphite paper tooling, and carbon fiber rope bundles are used to wrap and bundle the middle or three-division parts of the shaped graphite paper tooling to achieve fixation, and silicon powder is filled between the graphite paper tooling and the pre-connector to perform reactive infiltration, so that the preparation and connection of SiC-based ceramic materials are completed simultaneously, and a three-dimensional carbon fiber reinforced silicon carbide ceramic connector is obtained.
[0014] Preferably, the phenolic resin, ethylene glycol, benzenesulfonyl chloride, silicon carbide powder and graphite powder are mixed and stirred for 0.5 to 1 hour, filtered for 0.5 to 1 hour, and heated in a water bath to 50 to 70°C.
[0015] Preferably, the average particle size of the graphite powder is 30-40 μm; the average particle size of the silicon carbide powder is 1-2 μm.
[0016] Preferably, C f / C composite material is a continuous carbon fiber reinforced carbon matrix material, which is made by chemical vapor infiltration.
[0017] Preferably, C f The polished surface roughness of the connection surface of the / C composite material connection component is 7 to 13 μm.
[0018] Preferably, the staged curing is curing at a temperature of 70-80° C. for 2-3 hours, and then curing at a temperature of 150-160° C. for 8-10 hours.
[0019] Preferably, the carbonization is carried out in an argon atmosphere at a heating rate of 1 to 1.5° C. / min, at 800 to 1000° C., and kept warm for 2 to 4 hours.
[0020] Preferably, the pre-connector is wrapped with flexible graphite paper, and the graphite paper is cut, folded and assembled according to the three-dimensional structural shape of the pre-connector components, and a gap of 0.3 to 1 cm is left between the graphite paper and the pre-connector; the shaped graphite paper is fixed by wrapping it in the middle or in three equal parts by a carbon fiber rope bundle.
[0021] Preferably, the mass of the silicon powder is 1.5 to 2 times the mass of the pre-connector.
[0022] Preferably, the reactive infiltration is carried out at a vacuum degree of less than 10 Pa, a temperature of 1550-1650° C., and a heat preservation time of 40-60 min.
[0023] The present invention adopts the above technical solution, which has the following beneficial effects:
[0024] 1. The present invention uses flexible graphite paper to wrap the pre-connector and conducts three-dimensional reaction infiltration on the pre-connector, thereby solving the problems that the traditional silicon powder embedding method requires a large amount of silicon powder (according to the structure of the connector, the amount of silicon powder is usually 2 times or more of the preform), the insulation time is long, and the excess molten silicon is easy to solidify on the surface of the component during the cooling process, affecting the dimensional accuracy and requiring reprocessing. In addition, this method has been used to successfully prepare various density and high density pre-connector products at 1550℃ by adding 1.5 to 2 times the mass of the pre-connector and keeping it warm for 40 minutes.
[0025] 1.90g / cm 3 The above three-dimensional structural connectors are completely penetrated and have a net size. The connectors do not need to be polished or other subsequent processing steps, indicating that the method has a wide range of applications and strong operability.
[0026] 2. The present invention uses a flexible graphite paper tooling to control the distance between the graphite paper tooling and the preform (density is 1.45g / cm 3 , C with a cross-sectional size of 10mm×10mm f / C composite materials, the distance is controlled at 0.3-1cm), quantitative distribution of silicon powder is achieved, and silicon and pre-connectors are fully in contact in three dimensions. After heating, silicon melts, and silicon directly in contact with the pre-connectors enters the pre-connectors from each contact surface through capillary force, and Si-C reaction occurs, which effectively reduces the excessive reaction of silicon melt and carbon fiber in the traditional silicon powder embedding method, and can meet the requirements of some C / C composite materials that only need local ceramic modification.
[0027] 3. This method obtains a simple infiltration mold by folding graphite paper and fixing carbon fiber, which can replace customized graphite molds and effectively reduce production costs.
[0028] This method can realize the connection of SiC-based ceramic materials with three-dimensional structures, and the resulting connecting parts can be used in aerospace reflectors, automobile brake discs and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:
[0030] Figure 1 (a) and (b) are respectively the long strip C prepared in Example 1 f Schematic diagram of the C-SiC composite connector and the use of carbon fiber ropes to fix the shaped graphite paper;
[0031] Figure 2 (a) and (b) are respectively T-type C prepared in Example 2 f Schematic diagram of the C-SiC composite connector and the use of carbon fiber ropes to fix the shaped graphite paper;
[0032] Figure 3 (a) and (b) are three-dimensional I-shaped C prepared in Example 3. f Schematic diagram of the C-SiC composite connector and the use of carbon fiber ropes to fix the shaped graphite paper;
[0033] Figure 4 (a) and (b) are respectively the capless hexahedral C prepared in Example 4. f Schematic diagram of the C-SiC composite connector and the use of carbon fiber ropes to fix the shaped graphite paper;
[0034] Figure 5 (a) and (b) are backscattered electron morphology images of the connector when the amount of dissolved silicon powder is twice the mass of the connector: (a) 50×, (b) 1200×. DETAILED DESCRIPTION
[0035] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0036] An embodiment of the present invention provides a method for flexible wrapping synchronous reaction connection of a three-dimensional SiC-based ceramic material connector, comprising:
[0037] Step 1, phenolic resin, ethylene glycol, benzenesulfonyl chloride, silicon carbide powder and graphite powder are mixed and stirred in a mass ratio of 1:1:0.1:(0.1-0.2):(0.1-0.15) for 0.5-1h, transferred to a suction filtration bottle and filtered for 0.5-1h to remove bubbles, and heated in a water bath to 50-70°C to obtain a synchronous reaction connection slurry.
[0038] In step 1, the addition of graphite powder and silicon carbide powder can effectively inhibit the volume shrinkage and weight loss of the connection layer, and proper addition can improve the mechanical properties of the connection piece. The average particle size of the graphite powder is 30-40 μm, and the average particle size of the silicon carbide powder is 1-2 μm.
[0039] Step 2: C f The / C composite material is processed into the required size, and the surface to be connected is polished with sandpaper to keep the surface roughness at 7-13 μm.
[0040] In step 2, C f / C composite material is a continuous carbon fiber reinforced carbon matrix material, and the carbon fiber preform is made by chemical vapor infiltration (CVI). The roughness of the joint surface is maintained at 7-13μm to ensure that the slurry fully wets the joint surface.
[0041] Step 3, apply the prepared slurry to the connection surface with a blade, put it into an oven for curing at 70-80°C for 2-3 hours, and at 150-160°C for 8-10 hours after assembly. After curing, put the pre-connected parts into a tubular furnace and carbonize them under argon atmosphere at a heating rate of 1-1.5°C / min, a carbonization temperature of 800-1000°C, and keep them warm for 2-4 hours.
[0042] Step 4, cut and fold the graphite paper according to the shape of the pre-connector, wrap the pre-connector to form multiple graphite paper fixtures, leave a distance of 0.3-1cm between the graphite paper and the connector, so that it can be filled with 1.5 to 2 times the mass of the connector. Use carbon fiber rope bundles to wrap and bind the middle or three equal parts of the shaped graphite paper fixture to achieve fixation. Put the pre-connector and the graphite paper fixture into a graphite crucible, fill the pores between the two with silicon powder, and then put the whole into a vacuum siliconizing furnace. The reaction dissolution vacuum is below 10Pa, and the temperature is raised to 1550-1650℃ and kept warm for 40-60min. After cooling with the furnace, the connector is obtained.
[0043] In step 4, the three-dimensional contact between silicon particles and pre-connectors is achieved by coating with graphite paper flexible tooling. Compared with the traditional silicon powder embedding method, the amount of silicon powder used is greatly reduced, the construction period is shortened, and the difficulty of subsequent processing is reduced. By controlling the vacuum degree, the infiltration of silicon can be effectively promoted and the density of the connector can be increased.
[0044] In this method, based on the reaction connection, the pre-connected parts are wrapped with flexible graphite paper and fixed with carbon fiber rope bundles, thus achieving C f / C-SiC ceramic materials are connected by a three-dimensional synchronous reaction. The diverse three-dimensional structures enrich the use of this ceramic material, expand the application scope of the reaction infiltration process, reduce the tooling preparation cycle and cost, reduce the amount of silicon powder and reaction time of the three-dimensional structure connector, and shorten the construction period.
[0045] The present invention is further illustrated by means of specific examples below.
[0046] Example 1
[0047] Add phenolic resin, ethylene glycol, benzenesulfonyl chloride, SiC powder and graphite powder in the ratio of 10g:10g:1g:1g:1.1g into a suction flask, stir in a water bath at 60°C for 30 min, and vacuum filter and remove bubbles for 40 min to obtain resin slurry.
[0048] C f / C composite material is processed into two strips of 50mm×10mm×10mm, and the 10mm×10mm surface is polished with sandpaper to keep the surface roughness at 12μm, and used as the connection surface. The prepared slurry is applied to the connection surface with a blade, and after assembly, it is placed in an oven for curing at 80℃ for 2h and 150℃ for 9h. After curing, the pre-connector is placed in a tubular furnace and carbonized under an argon atmosphere at a carbonization temperature of 800℃ for 3h at a heating rate of 1℃ / min. After carbonization, the pre-connector is wrapped with cut and folded graphite paper as a whole, and the shaped graphite paper is wrapped and tied to the three equal parts vertically with a carbon fiber rope bundle. A gap of 0.3cm is left between the graphite paper and the connector so that it can be filled with 1.5 times the mass of the connector with silicon powder. The pre-connector and the graphite paper tooling were placed in a graphite crucible, the gap between the two was filled with silicon powder, and then the whole was placed in a vacuum siliconizing furnace, heated to 1550°C and kept warm for 40 minutes, and then cooled in the furnace to obtain a long strip connector. f The / C-SiC composite connector and the carbon fiber rope bundle used to fix the shaped graphite paper are shown in Figure 1(a) and (b).
[0049] By keeping the temperature for 40 min, a long strip of C f / C composite connector size is 100mm×10mm×10mm, density is 1.99g / cm 3 , open porosity is 3.63%, shear strength is 25.4MPa, and flexural strength is 29.23MPa. Figure 5 (a) is a backscattered electron morphology image of the connector at a magnification of 50 times. The black carbon phase, the white silicon phase, and the gray silicon carbide phase can be clearly seen. Figure 5 (b) The backscattered electron morphology image of the connector at a magnification of 1200 times shows that the carbon fiber remains intact and does not overreact, which is beneficial to maintaining the strength of the fiber.
[0050] Example 2
[0051] Add phenolic resin, ethylene glycol, benzenesulfonyl chloride, SiC powder and graphite powder in the ratio of 10g:10g:1g:1.5g:1g into a suction filtration bottle, stir in a water bath at 50°C for 50 minutes, and vacuum filter and remove bubbles for 30 minutes to obtain resin slurry.
[0052] C f / C composite materials were processed into strips of 60mm×10mm×10mm and 50mm×10mm×10mm. The 60mm×10mm surface of the former and the 10mm×10mm surface of the latter were polished with sandpaper to keep the surface roughness at 13μm, and used as the connection surface. The prepared slurry was applied to the connection surface with a blade, and after assembly, it was placed in an oven for curing at 70℃ for 3h and 150℃ for 10h. After curing, the pre-connector was placed in a tubular furnace and carbonized under an argon atmosphere. The carbonization temperature was 1000℃, the temperature was kept for 2h, and the heating rate was 1℃ / min. After carbonization, the upper and lower parts of the pre-connector were cut and folded for wrapping, and the two shaped graphite papers were wrapped and tied vertically in the middle with carbon fiber rope bundles. A gap of 0.4cm was left between the graphite paper and the connector so that it could be filled with silicon powder 1.75 times the mass of the connector. The pre-connector and the graphite paper tooling were placed in a graphite crucible, the gap between the two was filled with silicon powder, and then the whole was placed in a vacuum siliconizing furnace, heated to 1600°C and kept warm for 50 minutes, and then cooled in the furnace to obtain a T-shaped connector. f The / C-SiC composite connector and the carbon fiber rope bundle used to fix the shaped graphite paper are shown in Figure 2(a) and (b).
[0053] The T-type C was prepared by keeping the temperature for 50 min. f / C composite material connector density is 1.99g / cm 3 The open porosity is 4.63%, the material is composed of three phases of C, SiC and Si, the shear strength is 27.8 MPa, and the bending strength is 31.3 MPa. Other results are the same as those in Example 1.
[0054] Example 3
[0055] Add phenolic resin, ethylene glycol, benzenesulfonyl chloride, SiC powder and graphite powder in the ratio of 10g:10g:1g:1.5g:1.5g into a suction flask, stir in a water bath at 55°C for 60 minutes, and vacuum filter and remove bubbles for 60 minutes to obtain resin slurry.
[0056] C f / C composite material is processed into two 60mm×10mm×10mm strips and one 40mm×10mm×10mm strip. The 60mm×10mm surface of the former and the 10mm×10mm surface of the latter are polished with sandpaper to keep the surface roughness at 7μm, and used as the connection surface. The prepared slurry is applied to the connection surface with a blade, and after assembly, it is placed in an oven for curing at 80℃ for 2h and 160℃ for 8h. After curing, the pre-connector is placed in a tubular furnace and carbonized under an argon atmosphere. The carbonization temperature is 800℃, the temperature is kept for 4h, and the heating rate is 1.5℃ / min. After carbonization, the upper, middle and lower parts of the pre-connector are cut and folded for wrapping, and the three shaped graphite papers are wrapped and tied vertically in the middle with carbon fiber rope bundles. A gap of 0.6cm is left between the graphite paper and the connector so that it can be filled with silicon powder twice the mass of the connector. The pre-connector and the graphite paper tooling were placed in a graphite crucible, the gap between the two was filled with silicon powder, and then the whole was placed in a vacuum siliconizing furnace, heated to 1650°C and kept warm for 45 minutes, and then cooled in the furnace to obtain a three-dimensional I-shaped connector. f The / C-SiC composite connector and the use of carbon fiber ropes to fix the shaped graphite paper are shown in Figures 3(a) and (b).
[0057] The three-dimensional I-shaped C f / C composite material connector density is 2.01g / cm 3 The open porosity is 3.96%, the material is composed of three phases of C, SiC and Si, the shear strength is 31.9 MPa, and the bending strength is 43.7 MPa. Other results are the same as those in Example 1.
[0058] Example 4
[0059] Phenolic resin, ethylene glycol, benzenesulfonyl chloride, SiC powder and graphite powder were added into a suction filtration bottle in the ratio of 10g:10g:1g:2g:1.5g. The mixture was stirred in a water bath at 70°C for 45 min and vacuum filtered to remove bubbles for 50 min to obtain resin slurry.
[0060] C f / C composite material was processed into three 50mm×50mm×10mm squares and two 30mm×50mm×10mm strips. The 50mm×50mm surface of the former and the 30mm×50mm surface of the latter were polished with sandpaper to keep the surface roughness at 10μm, and used as the connection surface. The prepared slurry was applied to the connection surface with a blade, and after assembly, it was placed in an oven for curing at 70℃ for 2.5h and 150℃ for 10h. After curing, the pre-connector was placed in a tubular furnace and carbonized under an argon atmosphere. The carbonization temperature was 900℃, the temperature was kept for 4h, and the heating rate was 1℃ / min. After carbonization, the upper and lower parts of the pre-connector were cut and folded for wrapping, and the two shaped graphite papers were wrapped and tied vertically in the middle with carbon fiber rope bundles. A 1cm gap was left between the graphite paper and the connector so that it could be filled with silicon powder twice the mass of the connector, and the cavity was not filled with silicon powder. The pre-connector and the graphite paper tooling are placed in a graphite crucible, the gap between the two is filled with silicon powder, and then the whole is placed in a vacuum siliconizing furnace, heated to 1600°C and kept warm for 60 minutes, and then cooled in the furnace to obtain an uncovered hexahedral connector. f The / C-SiC composite connector and the carbon fiber rope bundle used to fix the shaped graphite paper are shown in Figures 4(a) and (b).
[0061] The capless hexahedral C f / C composite material connector density is 2.00g / cm 3 The open porosity is 3.93%, and the material is composed of three phases: C, SiC, and Si; and after adding water, the water does not leak, and has a certain sealing property. Other results are the same as those in Example 1.
[0062] It can be seen from the above embodiments that the method of the present invention achieves C f / C-SiC ceramic materials are connected by a one-time three-dimensional synchronous reaction. The amount of silicon powder required for the connecting parts is small, the insulation time is short, and the dimensional accuracy is high after the reaction and infiltration are completed. The density and open porosity of the prepared SiC-based ceramic composite connecting parts with different three-dimensional structures prove that the connecting parts have successfully completed the reaction and infiltration as a whole; and the obtained connecting parts have excellent mechanical properties, with a density of not less than 1.99g / cm3, an open porosity of not more than 4.63%, a shear strength of not less than 25.4MPa, and a flexural strength of not less than 29.23MPa.
[0063] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.
Claims
1. A method for flexible wrapping synchronous reaction connection of a three-dimensional SiC-based ceramic connector, characterized in that: The following steps are involved: Phenolic resin, ethylene glycol, benzenesulfonyl chloride, silicon carbide powder and graphite powder are mixed and stirred in a mass ratio of 1:1:0.1:(0.1-0.2):(0.1-0.15), filtered to remove bubbles, and heated in a water bath to obtain a synchronous reaction connection slurry; C f / C Polishing of the connection surface of composite material connection components; C f / C composite material connecting components are connected on the connecting surface by coating with reactive connecting slurry, assembling, curing in sections, and carbonizing to obtain a pre-connected component with a three-dimensional structure; Graphite paper is used to fold and wrap the pre-connected parts according to the shape of the pre-connected parts with a certain distance between the components. Carbon fiber rope bundles are used to wrap, bundle and fix the shaped graphite paper tooling. Silicon powder is filled between the graphite paper tooling and the pre-connected parts for reactive infiltration, so that the preparation and connection of SiC-based ceramic materials are completed simultaneously, and a three-dimensional carbon fiber reinforced silicon carbide ceramic connector is obtained.
2. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1 is characterized in that: Mix phenolic resin, ethylene glycol, benzenesulfonyl chloride, silicon carbide powder and graphite powder and stir for 0.5 to 1 hour, filter for 0.5 to 1 hour, and heat in a water bath to 50 to 70°C.
3. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: The average particle size of graphite powder is 30-40 μm; the average particle size of silicon carbide powder is 1-2 μm.
4. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: C f / C composite material is a continuous carbon fiber reinforced carbon matrix material, which is made by chemical vapor infiltration.
5. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: C f The polished surface roughness of the connection surface of the / C composite material connection component is 7 to 13 μm.
6. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: The staged curing is performed at a temperature of 70 to 80°C for 2 to 3 hours, and then at a temperature of 150 to 160°C for 8 to 10 hours.
7. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: The carbonization is carried out in an argon atmosphere at a heating rate of 1 to 1.5°C / min, at 800 to 1000°C, and kept warm for 2 to 4 hours.
8. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: The pre-connector is wrapped with flexible graphite paper, and the graphite paper is cut, folded and assembled according to the three-dimensional structural shape of the pre-connector components, and a gap of 0.3 to 1 cm is left between the graphite paper and the pre-connector; the middle or three-division of the shaped graphite paper is wrapped and fixed by carbon fiber rope bundles.
9. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: The mass of silicon powder is 1.5 to 2 times the mass of the pre-connector.
10. The method for flexible wrapping synchronous reaction connection of three-dimensional SiC-based ceramic connectors according to claim 1, characterized in that: The reaction infiltration is carried out at a vacuum degree below 10Pa, a temperature of 1550-1650°C, and a heat preservation time of 40-60 minutes.
Citation Information
Patent Citations
Online reaction connection method of ceramic blanks
CN104496511A
Reactive sintering Cf / SiC composite material and synchronous reaction connection method
CN108794041A
Melt siliconizing method for small-size circular-section ceramic-based composite material component
CN112341213A
Method for preparing C / SiC-Diamond composite material through RMI
CN116947515A
Method for preparing ceramic-based composite material through combination of precursor impregnation cracking and reactive infiltration
CN117534495A