A soft light brick with no bead effect on the bottom of the brick and a preparation method thereof

By using unglazed coarse tiles and water-based soft light anti-fouling liquid treatment during the preparation of soft light ceramic tiles, combined with nano-silicon sol filling, the problems of load bead effect and high cost are solved, and the load beadless effect on the brick bottom is achieved and Soft light ceramic tiles with excellent anti-fouling performance.

CN118724617BActive Publication Date: 2024-11-26GUANGDONG NADE NEW MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411233352.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-26
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The existing soft light ceramic tiles are prone to lot bead effect during the preparation process, resulting in no water on the bottom of the brick, affecting the laying and anti-fouling performance of the ceramic tiles, and the processing cost is high.

Method used

The unglazed coarse brick blank is used as the substrate, and the glossiness is controlled to be less than 30° by polishing and water-based soft light anti-fouling liquid treatment to form a transparent crystal film, combined with the nano-silicon sol filling and the use of water-based anti-fouling agent to avoid the load-beading effect and Improve anti-fouling performance.

Benefits of technology

The brick bottom is free of beads, which improves the soft light effect and anti-fouling ability, while reducing processing costs and improving the market recognition and shipment volume of products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a soft-light brick with no-bead effect on the bottom of a brick and a preparation method thereof, and relates to the field of ceramic tile processing. The preparation process comprises the following steps: (1) a brick blank selection step: selecting an unglazed rough brick blank as a substrate; (2) a rough brick blank surface repair step: adding a rough brick blank repair liquid, and using a polishing device to polish and repair the surface of the unglazed rough brick blank in step (1), and controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick blank is less than 30°; (3) a water-based soft-light anti-fouling treatment step: using a polishing device to drip and coat the surface of the unglazed rough brick blank with a repair layer with a water-based soft-light anti-fouling liquid, and polishing and coating. Compared with existing soft-light ceramic tile products, the soft-light brick with no-bead effect on the bottom of a brick prepared by the present invention can achieve excellent results in the soft-light effect of grinding head marks, anti-fouling ability, processing cost, and the no-bead effect on the bottom of the brick.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of soft light ceramic tile processing, and in particular to a soft light tile with no bead effect on the bottom of the tile and a preparation method thereof. Background Art

[0002] For a long time in the past, the "super-bright" ceramic tiles in the building ceramics industry have been favored by many consumers due to their super-high surface gloss, high hardness and good anti-fouling performance. However, super-bright ceramic tiles have a high reflectivity to light, which is easy to cause light pollution and visual fatigue. Therefore, with the continuous improvement of people's living standards, higher requirements are placed on the gloss of ceramic plates. In recent years, the market share of soft-light ceramic tiles with lower gloss has grown rapidly. There are three main ways to obtain a soft light effect on the surface of existing soft-light ceramic tiles:

[0003] One is to softly polish the glaze surface of the ceramic tile to a soft light to achieve a soft light effect. The polishing tools of this soft light process rub the glaze surface unevenly, leaving marks of the grinding head on the tile surface and destroying the crystal structure of the glaze. There will be tiny pores on the surface, which are easy to hide dirt and grime, and its anti-fouling performance is poor.

[0004] The second method is to apply a layer of specially adjusted soft-light glaze on the surface of the ceramic tile and adjust the glaze formula to reduce the glossiness of the glaze surface; however, the glaze research and development cost of this soft-light method is high.

[0005] Third, a layer of silicone oil-based water-based soft light anti-fouling liquid is applied on the surface of the ceramic tile to form a transparent crystalline film on the tile surface, increase the height and maintain the soft light effect; for example, patent CN202310461306.6 discloses a kind of anti-fouling soft light ceramic tile with unglazed rough brick as the matrix and its preparation method, which is specifically coated with a thin concentration and large particle size nano-silica sol on the unglazed rough brick, so that it adheres to the rough brick with no glaze on the surface, and can be adapted to fill and repair the coarse holes and cracks of the rough brick. Then, the repaired rough brick is coated with water-based soft light anti-fouling liquid for polishing, glazing and anti-fouling, which can form a transparent crystalline film on the brick surface, increase the height and maintain the soft light effect, and has excellent anti-fouling effect. However, since silicone oil-based water-based soft light anti-fouling liquid has excellent hydrophobicity, during the preparation process, the silicone oil anti-fouling agent will penetrate through the membrane to the bottom of the brick or during the coating process, splash onto the mechanical belt and then stick to the bottom of the brick, causing the bottom of the brick to be non-sticky, which is the so-called "lotus bead effect". The non-stickiness of the bottom of the brick will cause cement and other adhesive materials to fail to adhere when the tiles are laid, and the tiles will subsequently become hollow and fall off.

[0006] Therefore, it is urgent to develop an iteration such as patent CN202310461306.6 which discloses a kind of anti-fouling soft-light ceramic tile with unglazed rough brick as the base, so that it has soft light and anti-fouling effect. At the same time, the overall processing cost of the ceramic product is lower, and there is no lotus bead effect on the bottom of the product brick, which increases the product shipment volume and market recognition. Summary of the invention

[0007] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a soft-light brick with no bead effect on the bottom of the brick and a preparation method thereof. Compared with the existing soft-light ceramic tile products, the soft-light brick with no bead effect on the bottom of the brick produced by the present invention can achieve excellent results in the soft-light effect of grinding head marks, anti-fouling ability, processing cost, and no bead effect on the bottom of the brick.

[0008] One of the purposes of the present invention is achieved by adopting the following technical solution: a method for preparing a soft light brick with no bead effect on the bottom of the brick, comprising the following steps:

[0009] (1) Brick selection steps:

[0010] An unglazed rough brick is selected as the substrate. After polishing, the surface of the unglazed rough brick is smooth and the glossiness is less than 15°. The unglazed rough brick is a rough brick pressed by a press, and no glaze is applied to the surface of the rough brick.

[0011] (2) Steps for repairing the rough brick surface:

[0012] Adding a rough brick repair liquid, using a polishing device to polish and repair the surface of the unglazed rough brick selected in step (1), controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick is less than 30°;

[0013] (3) Water-based soft light anti-fouling treatment steps:

[0014] The water-based soft light antifouling liquid is continuously dripped and coated on the surface of the unglazed rough brick with the repair layer obtained in step (2) by using a polishing device, and the dripping speed and the polishing and coating time are controlled to form a layer of water-based soft light antifouling layer on the surface of the unglazed rough brick; the water-based soft light antifouling liquid comprises component A and component B, component A is a curing agent solution; the curing agent solution is a curing agent solution formed by mixing isobutyl triethoxy silane coupling agent and 120# solvent-based gasoline; component B is a water-based antifouling liquid; the water-based antifouling agent is a water-based antifouling liquid formed by mixing water glass, sodium hydroxymethyl cellulose, boric acid and water.

[0015] Optionally, in step (1), the unglazed rough brick is pre-treated by polishing its surface using a conventional polishing device equipped with elastic grinding blocks and fiber grinding blocks of different coarsenesses, so that its surface is smooth and the glossiness is controlled within 15°.

[0016] Optionally, in step (2), the rough brick repair liquid includes 1-2.5% by mass of large-particle silica sol with a particle size range of 180-195 nm and 1.5-2.5% by mass of large-particle silica sol with a particle size range of 130-145 nm; the silica sol is purchased from nano silica sol provided by Beijing Dekedaojin Technology Co., Ltd.

[0017] Optionally, in step (2), an ultra-clean polishing device is used, with soft fiber abrasive as the polishing medium; the rough brick blank repair liquid is dripped into and coated on the surface of the unglazed rough brick blank, the dripping speed and the polishing coating time are controlled to allow it to penetrate into the surface pores of the unglazed rough brick blank, and this is repeated twice; then clean water is dripped into the device for further polishing, the dripping speed and the polishing coating time are controlled to polish away the local agglomeration and uneven particles that appear during the repair process of the rough brick blank repair liquid, and this is repeated four times.

[0018] Optionally, in step (2), the amount of the rough brick repair liquid added is 2-6 g / m 2 The time for dripping the rough brick repair liquid is controlled at 15-25s, and the grinding and coating time is 55-80s; the revolution speed of the grinding disc of the super clean polishing equipment is 25-35r / min, and the rotation speed of the soft fiber abrasive installed on the grinding disc is 900-1000r / min; the amount of clean water added is 15-25g / m 2 ; The time for dripping clean water is controlled at 15-25s, and the time for grinding and coating is 20-45s; the revolution speed of the grinding disc of the ultra-clean and bright polishing equipment is 90-135r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 900-1000r / min.

[0019] Optionally, in step (3), the curing agent solution of component A is a curing agent solution mixed with a silane coupling agent and 120# solvent-based gasoline in a mass ratio of 1:(0.8-1.5); the aqueous antifouling liquid of component B; the aqueous antifouling agent comprises 3-8% by mass of water glass, 0.05-0.2% by mass of sodium hydroxymethyl cellulose and 0.5-1% by mass of boric acid.

[0020] Optionally, the preparation method of the aqueous antifouling liquid is as follows: before the aqueous soft light antifouling treatment, a formulated amount of water glass is added to a certain proportion of water, and the water glass is diluted by mixing and stirring at a speed of 550 r / min for 25 min; then a formulated amount of sodium hydroxymethyl cellulose is added to the diluted solution at a speed of 550 r / min for 10 min; finally, a formulated amount of boric acid is added and stirred to obtain an aqueous antifouling liquid.

[0021] Optionally, in step (3), an ultra-clean polishing device is used, with sponge abrasive as the polishing medium; the sponge abrasive in the ultra-clean nanomachine is used to quickly coat a layer of component B on the surface of the unglazed rough brick, and the component B penetrates into the fine pores on the surface of the unglazed rough brick and refills; then the sponge abrasive is used to coat a layer of component A on the surface of component B, and component A can be combined with component B in the previous step; finally, the sponge abrasive is used to coat another layer of component B on the surface of component A.

[0022] Optionally, the amount of component B added is 10-15 ml / m 2 The amount of component A added is 10-15 ml / m 2 ; The dropping time of component B is controlled at 8-10s, the grinding and coating time is 15-25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80-120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200-1400r / min; The dropping time of component A is controlled at 8-10s, the grinding and coating time is 15-25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80-120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200-1400r / min.

[0023] The second purpose of the present invention is achieved by adopting the following technical scheme: a soft light brick with no load bead effect on the bottom of the brick, characterized in that it is prepared by the preparation method of the soft light brick with no load bead effect on the bottom of the brick as described above.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] Compared with existing soft light ceramic tile products, the soft light brick with no bead effect on the bottom of the brick of the present invention can achieve excellent results in the soft light effect of grinding head marks, anti-fouling ability, processing cost and no bead effect on the bottom of the brick. The specific analysis is as follows: The present invention coats a nano-silica sol with a dilute concentration and large particle size on the unglazed rough brick blank, so that it adheres to the rough brick blank without glaze on the surface, and can adapt to fill and repair the coarse holes and cracks of the rough brick blank. In addition, in this step, the denser the nano material filling, the glossiness is controlled to be less than 30°, the better the polishing effect of the subsequent soft light anti-fouling process, the easier it is to increase the light, and improve the fineness of the soft light. Then, on the repaired rough brick blank, apply an aqueous soft light anti-fouling liquid for polishing, polishing and anti-fouling, which can form a layer of transparent crystalline film on the brick surface, increase the height and maintain the soft light effect, and the silicon crystalline film has an excellent anti-fouling effect, and there is no bead effect on the bottom of the brick. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0027] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0028] The present invention provides a method for preparing a soft light brick with no bead effect on the bottom of the brick, comprising the following steps:

[0029] (1) Brick selection steps:

[0030] An unglazed rough brick is selected as the substrate. After polishing, the surface of the unglazed rough brick is smooth and the glossiness is less than 15°. The unglazed rough brick is a rough brick pressed by a press, and no glaze is applied to the surface of the rough brick.

[0031] (2) Steps for repairing the rough brick surface:

[0032] Adding a rough brick repair liquid, using a polishing device to polish and repair the surface of the unglazed rough brick selected in step (1), controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick is less than 30°;

[0033] (3) Water-based soft light anti-fouling treatment steps:

[0034] The water-based soft light antifouling liquid is continuously dripped and coated on the surface of the unglazed rough brick with the repair layer obtained in step (2) by using a polishing device, and the dripping speed and the polishing and coating time are controlled to form a layer of water-based soft light antifouling layer on the surface of the unglazed rough brick; the water-based soft light antifouling liquid comprises component A and component B, component A is a curing agent solution; the curing agent solution is a curing agent solution formed by mixing isobutyl triethoxy silane coupling agent and 120# solvent-based gasoline; component B is a water-based antifouling liquid; the water-based antifouling agent is a water-based antifouling liquid formed by mixing water glass, sodium hydroxymethyl cellulose, boric acid and water.

[0035] As a further preferred embodiment, in step (1), the unglazed rough brick is pre-treated by polishing the surface using a conventional polishing device equipped with elastic grinding blocks and fiber grinding blocks of different coarsenesses, so that the surface is smooth and the glossiness is controlled within 15°.

[0036] As a further preferred embodiment, in step (2), the rough brick repair liquid includes 1-2.5% by mass of large-particle silica sol with a particle size range of 180-195 nm and 1.5-2.5% by mass of large-particle silica sol with a particle size range of 130-145 nm; the silica sol is purchased from nano silica sol provided by Beijing Dekedaojin Technology Co., Ltd.

[0037] As a further preferred embodiment, in step (2), an ultra-clean polishing device is used, with soft fiber abrasive as the polishing medium; the rough brick blank repair liquid is dripped into and coated on the surface of the unglazed rough brick blank, the dripping speed and the polishing coating time are controlled to allow it to penetrate into the surface pores of the unglazed rough brick blank, and this is repeated twice; then clean water is dripped into the polishing process, the dripping speed and the polishing coating time are controlled to polish away the local agglomeration and uneven particles that appear during the repair process of the rough brick blank repair liquid, and this is repeated four times.

[0038] As a further preferred embodiment, in step (2), the amount of the rough brick repair liquid added is 2-6 g / m 2 The time for dripping the rough brick repair liquid is controlled at 15-25s, and the grinding and coating time is 55-80s; the revolution speed of the grinding disc of the super clean polishing equipment is 25-35r / min, and the rotation speed of the soft fiber abrasive installed on the grinding disc is 900-1000r / min; the amount of clean water added is 15-25g / m 2 ; The time for dripping clean water is controlled at 15-25s, and the time for grinding and coating is 20-45s; the revolution speed of the grinding disc of the ultra-clean and bright polishing equipment is 90-135r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 900-1000r / min.

[0039] As a further preferred embodiment, in step (3), the curing agent solution of component A is a curing agent solution mixed with a silane coupling agent and 120# solvent-based gasoline in a mass ratio of 1:(0.8-1.5); the aqueous antifouling liquid of component B; the aqueous antifouling agent comprises 3-8% by mass of water glass, 0.05-0.2% by mass of sodium hydroxymethyl cellulose and 0.5-1% by mass of boric acid.

[0040] As a further preferred embodiment, the silane coupling agent is selected from the isobutyltriethoxysilane coupling agent provided by Jinan Rongzheng Chemical Co., Ltd.

[0041] As a further preferred embodiment, in step (3), an ultra-clean polishing device is used, with sponge abrasive as the polishing medium; the sponge abrasive in the ultra-clean nanomachine is used to quickly coat a layer of component B on the surface of the unglazed rough brick, and the component B penetrates into the fine pores on the surface of the unglazed rough brick and refills them; then, the sponge abrasive is used to coat a layer of component A on the surface of component B, and component A can be combined with component B in the previous step; finally, the sponge abrasive is used to coat another layer of component B on the surface of component A.

[0042] As a further preferred embodiment, the addition amount of component B is 10-15 ml / m 2 The amount of component A added is 10-15 ml / m 2; The dropping time of component B is controlled at 8-10s, the grinding and coating time is 15-25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80-120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200-1400r / min; The dropping time of component A is controlled at 8-10s, the grinding and coating time is 15-25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80-120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200-1400r / min.

[0043] The present invention also provides a soft-light brick with no lotus bead effect on the bottom of the brick, which is prepared by the preparation method of the soft-light brick with no lotus bead effect on the bottom of the brick.

[0044] The following are specific embodiments of the present invention. Unless otherwise specified, the raw materials, equipment, etc. used in the following embodiments can be obtained by purchase.

[0045] According to the formula in Table 1-2 below, each component was taken, and a rough brick repair liquid and an aqueous soft light antifouling liquid were prepared according to the following preparation methods for use in various embodiments.

[0046] Table 1 is the formula composition of the rough brick repair liquid of each embodiment

[0047]

[0048] Note: The silica sol described in Table 1 was purchased from nano silica sol provided by Beijing Dekedaojin Technology Co., Ltd.

[0049] Table 2 shows the formula composition of the water-based soft light antifouling liquid of each embodiment

[0050]

[0051] Note: The silane coupling agent described in Table 2 is selected from the isobutyl triethoxy silane coupling agent provided by Jinan Rongzheng Chemical Co., Ltd., and the gasoline is 120# solvent-based gasoline. Water glass was purchased from Guangdong Huihe Silicon Products Co., Ltd., and its liquid water glass with a sodium oxide and silicon dioxide content of ≥35% was purchased from Guangdong Huihe Silicon Products Co., Ltd., sodium hydroxymethyl cellulose was purchased from Shandong Weifang Lit Composite Materials Co., Ltd., and boric acid was purchased from Henan Yiquan Chemical Technology Co., Ltd.

[0052] The preparation method of rough brick repair liquid is as follows: add the formulated amount of silica sol with different particle size ranges and water into the dispersion tank, start stirring, the stirring speed is 380r / min, and the stirring time is 28min; then use a grinder to grind until there are no coarse particles, the speed is 500r / min, and the grinding time is 6min.

[0053] The preparation method of the curing agent solution is as follows: before the soft light antifouling treatment, the silane coupling agent and 120# solvent gasoline are taken in the formula amount, and the silane coupling agent and 120# solvent gasoline are mixed and stirred at a stirring speed of 350r / min and a stirring time of 10min; finally, the curing agent solution is obtained;

[0054] The preparation method of the water-based antifouling liquid is as follows: before the water-based soft light antifouling treatment, add a formulated amount of water glass to a certain proportion of water, mix and stir to dilute the water glass, the stirring speed is 550r / min, and the stirring time is 25min; then add the formulated amount of sodium hydroxymethyl cellulose and the remaining water into the diluted solution to increase the hardness after crystallization, the stirring speed is 550r / min, and the stirring time is 10min; finally, add the formulated amount of boric acid and stir to lower the pH value of the system to avoid excessive alkalinity of the solution system and cause corrosion of the brick surface, and finally obtain the water-based antifouling liquid.

[0055] Examples 1-3 and Comparative Examples 1-8

[0056] Among them, the soft light bricks of Examples 1-3 and Comparative Examples 1-6 are selected from the same batch of unglazed rough bricks produced by a company on the market. The unglazed rough bricks are rough bricks pressed by a press, and the rough bricks are not glazed on the surface of the rough bricks. The unglazed rough bricks are surface treated according to the preparation processes of Examples 1-3 and Comparative Examples 1-6. Comparative Examples 7-8 are existing common soft light brick products, purchased from different ceramic manufacturers.

[0057] Example 1

[0058] A soft light brick with no bead effect on the bottom of the brick, the preparation method of which comprises the following steps:

[0059] (1) Brick selection steps:

[0060] Unglazed rough bricks are selected as the substrate. After polishing, the surface of the unglazed rough bricks is smooth and the glossiness is less than 15°. Specifically, the unglazed rough bricks are rough bricks pressed by a press and pre-polished by conventional polishing equipment equipped with elastic grinding blocks and fiber grinding blocks of different coarsenesses to make their surfaces smooth and the glossiness is controlled within 15°.

[0061] (2) Steps for repairing the rough brick surface:

[0062] Adding a rough brick repair liquid, using a polishing device to polish and repair the surface of the unglazed rough brick selected in step (1), controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick is less than 30°; using an ultra-clean polishing device and using a sponge abrasive as a polishing medium;

[0063] Specifically, the rough brick repair liquid is dripped into and coated on the surface of the unglazed rough brick after treatment in step (1), and the dripping speed and the grinding and coating time are controlled to make it penetrate into the surface pores of the unglazed rough brick, and this is repeated twice; then clean water is dripped into and the grinding is continued, and the dripping speed and the grinding and coating time are controlled to grind off the local agglomeration and uneven particles that appear in the repair process of the rough brick repair liquid, and this is repeated four times.

[0064] The amount of the rough brick repair liquid added is 3g / m 2 The time of dripping the rough brick repair liquid is controlled at 15s, and the grinding and coating time is 55s; the revolution speed of the grinding disc of the super clean polishing equipment is 25r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 900r / min; the amount of clean water added is 15g / m 2 ; The time for dripping clean water is controlled at 15s, and the time for polishing and coating is 20s; the revolution speed of the grinding disc of the ultra-clean and bright polishing equipment is 90r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 900r / min.

[0065] (3) Water-based soft light anti-fouling treatment steps:

[0066] The polishing equipment is used to drip and apply the water-based soft light antifouling liquid on the surface of the unglazed rough brick with the repair layer obtained in step (2), and the dripping speed and polishing coating time are controlled to form a water-based soft light antifouling layer on the surface of the unglazed rough brick. The ultra-clean polishing equipment is used, and the sponge abrasive is used as the polishing medium; the sponge abrasive in the ultra-clean nano machine is used to quickly apply a layer of component B on the surface of the unglazed rough brick, and the component B penetrates into the fine pores on the surface of the unglazed rough brick and refills; then the sponge abrasive is used to apply a layer of component A on the surface of the component B, and the component A can be combined with the component B in the previous step; finally, the sponge abrasive is used to apply another layer of component B on the surface of the component A.

[0067] The addition amount of the B component is 10ml / m 2 The amount of component A added is 10 ml / m 2 ; The dropping time of component B is controlled at 8s, the grinding and coating time is 15s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200r / min; The dropping time of component A is controlled at 8s, the grinding and coating time is 15s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200r / min.

[0068] Example 2

[0069] A soft light brick with no bead effect on the bottom of the brick, the preparation method of which comprises the following steps:

[0070] (1) Brick selection steps:

[0071] Unglazed rough bricks are selected as the substrate. After polishing, the surface of the unglazed rough bricks is smooth and the glossiness is less than 15°. Specifically, the unglazed rough bricks are rough bricks pressed by a press and pre-polished by conventional polishing equipment equipped with elastic grinding blocks and fiber grinding blocks of different coarsenesses to make their surfaces smooth and the glossiness is controlled within 15°.

[0072] (2) Steps for repairing the rough brick surface:

[0073] Adding a rough brick repair liquid, using a polishing device to polish and repair the surface of the unglazed rough brick selected in step (1), controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick is less than 30°; using an ultra-clean polishing device and using a sponge abrasive as a polishing medium;

[0074] Specifically, the rough brick repair liquid is dripped into and coated on the surface of the unglazed rough brick after treatment in step (1), and the dripping speed and the grinding and coating time are controlled to make it penetrate into the surface pores of the unglazed rough brick, and this is repeated twice; then clean water is dripped into and the grinding is continued, and the dripping speed and the grinding and coating time are controlled to grind off the local agglomeration and uneven particles that appear in the repair process of the rough brick repair liquid, and this is repeated four times.

[0075] The amount of the rough brick repair liquid added is 5g / m 2 The time of dripping the rough brick repair liquid is controlled at 20s, and the grinding and coating time is 65s; the revolution speed of the grinding disc of the super clean polishing equipment is 30r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 950r / min; the amount of clean water added is 20g / m 2 ; The time for dripping clean water is controlled at 20s, and the time for polishing and coating is 35s; the revolution speed of the grinding disc of the ultra-clean and bright polishing equipment is 105r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 950r / min.

[0076] (3) Water-based soft light anti-fouling treatment steps:

[0077] The polishing equipment is used to drip and apply the water-based soft light antifouling liquid on the surface of the unglazed rough brick with the repair layer obtained in step (2), and the dripping speed and polishing coating time are controlled to form a water-based soft light antifouling layer on the surface of the unglazed rough brick. The ultra-clean polishing equipment is used, and the sponge abrasive is used as the polishing medium; the sponge abrasive in the ultra-clean nano machine is used to quickly apply a layer of component B on the surface of the unglazed rough brick, and the component B penetrates into the fine pores on the surface of the unglazed rough brick and refills; then the sponge abrasive is used to apply a layer of component A on the surface of the component B, and the component A can be combined with the component B in the previous step; finally, the sponge abrasive is used to apply another layer of component B on the surface of the component A.

[0078] The amount of component B added is 12 ml / m 2 The amount of component A added is 12 ml / m 2 ; The dropping time of component B is controlled at 9s, the grinding and coating time is 20s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 105r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1300r / min; The dropping time of component A is controlled at 9s, the grinding and coating time is 20s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 105r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1300r / min.

[0079] Example 3

[0080] A soft light brick with no bead effect on the bottom of the brick, the preparation method of which comprises the following steps:

[0081] (1) Brick selection steps:

[0082] Unglazed rough bricks are selected as the substrate. After polishing, the surface of the unglazed rough bricks is smooth and the glossiness is less than 15°. Specifically, the unglazed rough bricks are rough bricks pressed by a press and pre-polished by conventional polishing equipment equipped with elastic grinding blocks and fiber grinding blocks of different coarsenesses to make their surfaces smooth and the glossiness is controlled within 15°.

[0083] (2) Steps for repairing the rough brick surface:

[0084] Adding a rough brick repair liquid, using a polishing device to polish and repair the surface of the unglazed rough brick selected in step (1), controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick is less than 30°; using an ultra-clean polishing device and using a sponge abrasive as a polishing medium;

[0085] Specifically, the rough brick repair liquid is dripped into and coated on the surface of the unglazed rough brick after treatment in step (1), and the dripping speed and the grinding and coating time are controlled to make it penetrate into the surface pores of the unglazed rough brick, and this is repeated twice; then clean water is dripped into and the grinding is continued, and the dripping speed and the grinding and coating time are controlled to grind off the local agglomeration and uneven particles that appear in the repair process of the rough brick repair liquid, and this is repeated four times.

[0086] The amount of the rough brick repair liquid added is 6g / m 2 The time of dripping the rough brick repair liquid is controlled at 25s, and the grinding and coating time is 80s; the revolution speed of the grinding disc of the super clean polishing equipment is 35r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1000r / min; the amount of clean water added is 25g / m 2; The time for dripping clean water is controlled at 25s, and the time for grinding and coating is 45s; the revolution speed of the grinding disc of the ultra-clean and bright polishing equipment is 135r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1000r / min.

[0087] (3) Water-based soft light anti-fouling treatment steps:

[0088] The polishing equipment is used to drip and apply the soft light antifouling liquid on the surface of the unglazed rough brick with the repair layer obtained in step (2), and the dripping speed and polishing coating time are controlled to form a water-based soft light antifouling layer on the surface of the unglazed rough brick. The ultra-clean polishing equipment is used, and the sponge abrasive is used as the polishing medium; the sponge abrasive in the ultra-clean nano machine is used to quickly apply a layer of component B on the surface of the unglazed rough brick, and the component B penetrates into the fine pores on the surface of the unglazed rough brick and refills; then the sponge abrasive is used to apply a layer of component A on the surface of the component B, and the component A can be combined with the component B in the previous step; finally, the sponge abrasive is used to apply another layer of component B on the surface of the component A.

[0089] The amount of component B added is 15 ml / m 2 The amount of component A added is 15 ml / m 2 ; The dropping time of component B is controlled at 10s, the grinding and coating time is 25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1400r / min; The dropping time of component A is controlled at 10s, the grinding and coating time is 25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1400r / min.

[0090] Comparative Example 1

[0091] The difference between Comparative Example 1 and Example 2 is that in step (3), an oily antifouling liquid is used instead of an aqueous antifouling liquid, wherein the formula and preparation method of the oily antifouling liquid refer to the oily antifouling liquid of Example 2 of the antifouling soft light ceramic tile instruction manual of Patent No. CN202310461306.6.

[0092] Comparative Example 2

[0093] The difference between Comparative Example 2 and Example 2 is that in the formulation of the aqueous antifouling liquid in step (3), the mass percentage of water glass exceeds the upper limit of the amount used in the present invention (3-8%) and is 10%, and the remaining steps, conditions and reagent formulations used are basically the same as those in Example 2.

[0094] Comparative Example 3

[0095] The difference between Comparative Example 3 and Example 2 is that in the formulation of the aqueous antifouling liquid in step (3), the mass percentage of water glass is less than the lower limit of the amount used in the present invention (3-8%), which is 2%, and the remaining steps, conditions and reagent formulations used are basically the same as those in Example 2.

[0096] Comparative Example 4

[0097] The difference between Comparative Example 4 and Example 2 is that the amount of sodium hydroxymethyl cellulose used in the formulation of the aqueous antifouling liquid in step (3) is 0, and the remaining steps, conditions and reagent formulations used are basically the same as those in Example 2.

[0098] Comparative Example 5

[0099] The difference between Comparative Example 5 and Example 2 is that the amount of boric acid used in the formulation of the aqueous antifouling liquid in step (3) is 0, and the remaining steps, conditions and reagent formulations used are basically the same as those in Example 2.

[0100] Comparative Example 6

[0101] The difference between Comparative Example 6 and Example 2 is that the preparation method of the aqueous antifouling liquid in step (3) is different, and the remaining steps, conditions and reagent formula used are basically the same as those in Example 2.

[0102] The preparation method of the water-based antifouling liquid in step (3) of comparative example 6 is as follows: before the water-based soft light antifouling treatment, the formulated amount of water glass, sodium hydroxymethyl cellulose and boric acid are directly mixed together, the stirring speed is 550 r / min, the stirring time is 35 min, and finally the water-based antifouling liquid is obtained.

[0103] Comparative Example 7

[0104] The existing soft-light ceramic tiles with a glaze layer are soft-light brick finished products purchased from Zhuhai Baitu Ceramics Co., Ltd. The general process of the soft-light brick is to apply conventional glaze on the surface of the brick blank, and then soft-polish the glaze surface of the ceramic tile using a conventional soft-polishing process.

[0105] Comparative Example 8

[0106] The existing soft-light ceramic tiles with a glaze layer are purchased from the soft-light brick finished products provided by Guangdong Dongpeng Holdings Co., Ltd. The soft-light bricks are generally obtained by applying a layer of soft-light glaze on the surface of the brick.

[0107] Effect evaluation and performance testing

[0108] 1. The performance of the soft light ceramic tiles of Examples 1-3 and Comparative Examples 1-8 was tested, and the grinding head marks, glossiness, and anti-fouling ability on the surface of the soft light ceramic tiles were tested, wherein the performance test items include glossiness, anti-fouling ability, and grinding head marks on the surface of the soft light ceramic tiles. The glossiness was tested according to GB / T13891-2008 standard. The test items and results are shown in Table 3 below; anti-fouling ability refers to the use of red, blue, and black pens to paint on the surface of the ceramic tile. After the handwriting is fully dried, it is washed with detergent water to observe whether it is cleaned. It is divided into multiple levels according to the degree of cleanliness. In addition, the cost mainly includes the sum of the cost of rough brick repair liquid, the cost of soft light anti-fouling liquid, the cost of glaze, and the cost of processing electricity. The brick bottom lotus bead effect refers to dripping water on the bottom surface of the ceramic tile obtained in each embodiment, observing the water droplets, and if water droplets are formed, there is a lotus bead effect. If water droplets are not formed, there is no lotus bead effect.

[0109] Table 3 is the performance test results of the soft light ceramic tiles of Examples 1-3 and Comparative Examples 1-8

[0110]

[0111] It can be seen from the above table that compared with the existing soft light ceramic tile products of comparative examples 7-8, the soft light bricks with no bead effect on the brick bottom of embodiments 1-3 can achieve excellent results in the soft light effect of grinding head marks, anti-fouling ability, processing cost and no bead effect on the brick bottom, especially embodiment 2, the soft light bricks with no bead effect on the brick bottom have soft light effect, excellent anti-fouling ability, no grinding head marks, the lowest processing cost, and no bead effect on the brick bottom, which is the optimal implementation method.

[0112] Compared with Example 2, Comparative Example 1 uses an oily antifouling liquid instead of an aqueous antifouling liquid, so that the bottom of the brick is not stained with water, and a lotus bead effect is produced. When the tiles are laid, adhesive materials such as cement cannot adhere to the bottom of the brick.

[0113] Compared with Example 2, in the formulation of the aqueous antifouling liquid in step (3), the mass percentage of water glass in Comparative Example 2-3 is not within the dosage range of 3-8% of the present invention. Water glass has a relatively high viscosity. When excessive water glass is added and polished, local agglomeration occurs on the surface of the brick body, affecting the visual effect. Insufficient water glass causes the antifouling of the tile to deteriorate, and the microscopic pores are not fully filled. It can be seen that excessive or small amounts of water glass cannot form an adhesiveness that satisfies the combination of the base material on the ceramic substrate and form a transparent crystalline film on the brick surface to increase the brightness and maintain the soft light effect.

[0114] Compared with Example 2, in the formulation of the aqueous antifouling liquid in step (3), Comparative Example 4 lacks sodium hydroxymethyl cellulose, and the filler has insufficient crystal density, which reduces the strength of the water glass cured film and deteriorates the luminosity and antifouling performance.

[0115] Compared with Example 2, in the formulation of the aqueous antifouling liquid in step (3) of Comparative Example 5, boric acid is lacking, and the alkalinity of the system is too strong, which makes it easy for the molecules to agglomerate without being dispersed. Adding boric acid as a slow-release material can prevent the corrosion rate of the water glass strong alkaline material on the brick surface, resulting in the so-called burning or indispersible situation.

[0116] Compared with Example 2, in Comparative Example 6, the preparation method of the aqueous antifouling liquid in step (3) is different. Water glass, sodium hydroxymethyl cellulose and boric acid are directly mixed together. Due to the excessive reaction of alkaline water glass and boric acid, silicate precipitation is formed in local areas, affecting the stability of the product system.

[0117] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for preparing a soft light brick with no bead effect on the bottom of the brick, characterized in that: The steps include: (1) Brick selection steps: An unglazed rough brick is selected as the substrate. After polishing, the surface of the unglazed rough brick is smooth and the glossiness is less than 15°. The unglazed rough brick is a rough brick pressed by a press, and no glaze is applied to the surface of the rough brick. (2) Steps for repairing the rough brick surface: Adding a rough brick repair liquid, using a polishing device to polish and repair the surface of the unglazed rough brick selected in step (1), controlling the polishing and coating time so that the glossiness of the surface of the unglazed rough brick is less than 30°; (3) Water-based soft light anti-fouling treatment steps: The water-based soft light antifouling liquid is continuously dripped and coated on the surface of the unglazed rough brick with the repair layer obtained in step (2) by using a polishing device, and the dripping speed and the polishing and coating time are controlled to form a water-based soft light antifouling layer on the surface of the unglazed rough brick; the water-based soft light antifouling liquid comprises a component A and a component B, wherein the component A is a curing agent solution; the curing agent solution is a curing agent solution formed by mixing an isobutyl triethoxysilane coupling agent with 120# solvent-based gasoline; and the component B is a water-based antifouling liquid; The aqueous antifouling liquid is a mixture of water glass, sodium hydroxymethyl cellulose, boric acid and water; In step (3), the curing agent solution of component A is a curing agent solution mixed with silane coupling agent and 120# solvent gasoline in a mass ratio of 1: (0.8-1.5); the aqueous antifouling liquid of component B; The aqueous antifouling liquid comprises 3-8% by mass of water glass, 0.05-0.2% by mass of sodium hydroxymethyl cellulose and 0.5-1% by mass of boric acid; The preparation method of the water-based antifouling liquid is as follows: before the water-based soft light antifouling treatment, a formulated amount of water glass is added to a certain proportion of water, and the water glass is diluted by mixing and stirring at a stirring speed of 550 r / min and a stirring time of 25 min; then a formulated amount of sodium hydroxymethyl cellulose is added to the diluted solution at a stirring speed of 550 r / min and a stirring time of 10 min; finally, a formulated amount of boric acid is added and stirred to obtain the water-based antifouling liquid.

2. The method for preparing the soft light brick with no bead effect on the bottom of the brick as claimed in claim 1, characterized in that: In step (1), the unglazed rough brick is pre-treated by polishing the surface using a conventional polishing device equipped with elastic grinding blocks and fiber grinding blocks of different coarsenesses, so that the surface is smooth and the glossiness is controlled within 15°.

3. The method for preparing the soft light brick with no bead effect on the bottom of the brick as claimed in claim 1, characterized in that: In step (2), the rough brick repair liquid includes 1-2.5% by mass of large-particle silica sol with a particle size range of 180-195 nm and 1.5-2.5% by mass of large-particle silica sol with a particle size range of 130-145 nm.

4. The method for preparing the soft light brick with no bead effect on the bottom of the brick as claimed in claim 1, characterized in that: In step (2), an ultra-clean polishing device is used, and soft fiber abrasive is used as the polishing medium; the rough brick blank repair liquid is dripped into and coated on the surface of the unglazed rough brick blank, and the dripping speed and the polishing coating time are controlled to allow it to penetrate into the surface pores of the unglazed rough brick blank, and this is repeated twice; then clean water is dripped into the device for further polishing, and the dripping speed and the polishing coating time are controlled to polish away the local agglomeration and uneven particles that appear during the repair process of the rough brick blank repair liquid, and this is repeated four times.

5. The method for preparing the soft light brick with no bead effect on the bottom of the brick as claimed in claim 4, characterized in that: In step (2), the amount of the rough brick repair liquid added is 2-6 g / m 2 The time for dripping the rough brick repair liquid is controlled at 15-25s, and the grinding and coating time is 55-80s; the revolution speed of the grinding disc of the super clean polishing equipment is 25-35r / min, and the rotation speed of the soft fiber abrasive installed on the grinding disc is 900-1000r / min; the amount of clean water added is 15-25g / m 2 ; The time for dripping clean water is controlled at 15-25s, and the time for grinding and coating is 20-45s; the revolution speed of the grinding disc of the ultra-clean and bright polishing equipment is 90-135r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 900-1000r / min.

6. The method for preparing the soft light brick with no bead effect on the bottom of the brick as claimed in claim 1, characterized in that: In step (3), an ultra-clean polishing device is used, with sponge abrasive as the polishing medium; a layer of component B is quickly coated on the surface of the unglazed rough brick blank using the sponge abrasive in the ultra-clean nanomachine, and the component B penetrates into the fine pores on the surface of the unglazed rough brick blank and refills; then a layer of component A is continuously coated on the surface of component B using the sponge abrasive, and component A can be combined with component B in the previous step; finally, a layer of component B is continuously coated on the surface of component A using the sponge abrasive.

7. The method for preparing the soft light brick with no bead effect on the bottom of the brick as claimed in claim 6, characterized in that: The addition amount of the B component is 10-15ml / m 2 The amount of component A added is 10-15 ml / m 2 ; The dropping time of component B is controlled at 8-10s, the grinding and coating time is 15-25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80-120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200-1400r / min; The dropping time of component A is controlled at 8-10s, the grinding and coating time is 15-25s, the revolution speed of the grinding disc of the super clean and bright polishing equipment is 80-120r / min, and the rotation speed of the sponge abrasive installed on the grinding disc is 1200-1400r / min.

8. A soft light brick with no bead effect on the bottom of the brick, characterized in that: The brick is prepared by the method for preparing the soft light brick with no bead effect on the bottom of the brick as described in any one of claims 1 to 7.