Nano silicon-rich mineral powder as well as preparation method and application thereof

Through the compounding and hydrothermal reaction of sticky rocks, phosphate rocks and potassium-rich rocks, nano-silica-rich mineral powder is prepared, which solves the problem of potassium minerals being difficult to absorb by plants, improves the extraction rate of potassium and phosphorus, and improves the soil improvement effect. Significantly improved crop yield and disease resistance.

CN118724629APending Publication Date: 2024-10-01BANSHISHI SPECIAL FERTILIZER RES & DESIGN INST (HENAN) CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410943236.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, water-insoluble potassium mineral is difficult to be absorbed by plants, and after extraction, it combines with calcium to form a precipitate, which cannot be utilized by plants, resulting in poor application effects.

Method used

Using a compounding method of sticky rocks, phosphate rocks and potassium-rich rocks, nano-silica-rich mineral powder is prepared through hydrothermal reaction. Surfactants are used to improve the wettability and extraction rate of the ores to ensure that the mass fraction of sticky rocks is greater than The total mass fraction of phosphate rock and potassium-rich rock is subjected to a hydrothermal reaction of 0.4 to 0.6Mpa at a temperature of 165 to 255°C to generate two-dimensional mineral silicon flake materials with a fineness of 17 to 56 nanometers.

Benefits of technology

It significantly improves the extraction rate of potassium and phosphorus, increases the contact area between ore and water, increases the potassium and phosphorus content that plants can absorb, improves soil structure and crop yield, and improves disease resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to nano silicon-rich mineral powder as well as a preparation method and application thereof, and is characterized in that the nano silicon-rich mineral powder is prepared by grinding cohesive stone, ground phosphate rock and potassium-rich rock and then carrying out hydrothermal reaction, the mass fraction of the cohesive stone is greater than the total mass fraction of the ground phosphate rock and the potassium-rich rock. The method can improve the extraction rate of citrate soluble phosphorus in the ground phosphate rock and the extraction rate of potassium in the potassium-rich rock, and can be used in soil or fertilizers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to nano silicon-rich ore powder and a preparation method and application thereof. Background Art

[0002] my country lacks soluble potash resources, but has abundant water-insoluble potash resources. How to convert water-insoluble potash into potassium that can be absorbed by plants has become a research direction. At present, the hydrothermal method of the Institute of Geology and Geophysics, Chinese Academy of Sciences, such as patent number CN 104844302, is a method for producing multi-element microporous mineral fertilizer (soil conditioner) of phosphorus, potassium, silicon and calcium. It uses a mixture of potassium-rich rock, lime and phosphate rock, and reacts for 8h to 24h under saturated steam pressure of 160℃-250℃. In terms of the detection method, it adopts weighing 1.0000g of the dried product sample, placing it in a 300ml triangular flask, adding 100ml of 0.5mol / l hydrochloric acid solution, covering the bottle stopper, and placing it in an oscillator for half an hour. Hydrochloric acid is a strong acid, and when applied to plants, the root system of the plant can only secrete organic acid, which cannot reach the strong acid standard. Therefore, there is a problem that the extraction rate is high, but the actual crop cannot absorb it, and the application effect is poor. Take silicon as an example. Since its mineral mixture contains a large amount of calcium, even if the silicon is extracted, it will eventually combine with calcium to form calcium silicate or calcium metasilicate precipitates. Although these can be detected, they cannot be used by plants, so the effect is not good.

[0003] Nanofertilizer has a large specific surface area and can improve the soil better when applied to the soil, which has become a research direction.

[0004] Currently, there is no product or method that has a high mineral extraction rate and good practical application effect, nor is there a product or method that can better improve the soil. Summary of the invention

[0005] The invention provides a nano silicon-rich ore powder and a preparation method and application thereof, which solve the technical problem that potassium is difficult to extract from potassium-rich rocks and the application effect after extraction is not good.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions: A nano silicon-rich ore powder is obtained by grinding clay stone, phosphate ore and potassium-rich rock, and subjecting them to hydrothermal reaction; the mass fraction of the clay stone is greater than the total mass fraction of the phosphate ore and the potassium-rich rock.

[0007] The clay stone is one or both of kaolinite and illite; the potassium-rich rock is one or both of mica and potassium feldspar.

[0008] 50-60 parts of kaolinite, 10-15 parts of phosphate rock, 20-30 parts of illite, and 40-60 parts of potassium-rich rock, and the total mass fraction of kaolinite and illite is greater than the total mass fraction of phosphate rock and potassium-rich rock.

[0009] The hydrothermal reaction temperature is 165-255° C., the pressure is 0.4-0.6 MPa, and the pH is 8.0-10.

[0010] The preparation method of nano silicon-rich ore powder is carried out according to the following steps: S1. Initial stage of crushing: put clay stone, phosphate rock and potassium-rich rock into ore crusher and crush them into 15-20 mesh. Mix well to obtain silicon-rich ore powder A; S2, further grinding and crushing the silicon-rich ore powder A to 170-200 mesh to obtain silicon-rich ore powder B; S3, adding water and surfactant to the silicon-rich mineral powder B, stirring evenly, and then grinding in a sand mill until the mineral powder fineness is 2 to 20 microns, which is recorded as silicon-rich mineral dispersion C; S4, transfer the silicon-rich mineral dispersion C into a reactor, add 1 to 3 times of water, and perform hydrothermal reaction at a temperature of 165 to 255°C and a pressure of 0.4 to 0.6 MPa for 16 to 24 hours to obtain a slurry, blow out the slurry while it is hot through an air flow, collect and cool it, and obtain fluffy silicon-rich mineral powder; S5. The fluffy silicon-rich ore powder is crushed by a jet mill to obtain a two-dimensional mineral silicon flake material with a fineness of 17 to 56 nanometers, namely, nano silicon-rich ore powder.

[0011] The surfactant is one or a mixture of two or more of sodium hexametaphosphate, sodium pyrophosphate, sodium polyacrylate, triethanolamine, sodium lignin sulfonate, sodium naphthalene sulfonate and alkylphenol polyoxyethylene ether.

[0012] In step S3, the mass ratio of silicon-rich ore powder B: water: surfactant is 100:30-40:0.2-2.

[0013] Application of nano silicon-rich mineral powder: fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder as soil conditioner, directly applied to the soil; or The fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a fertilizer additive and applied to fertilizers.

[0014] The invention has the following beneficial technical effects: 1. The thickness of the nano silicon-rich ore powder prepared in this application is between 10-150nm, and it has a large specific surface area, which is 18.793m 2 / g.

[0015] 2. The present application compounds clay stone, phosphate rock and potassium-rich rock, and limits the mass fraction of clay stone to be greater than the total mass fraction of phosphate rock and potassium-rich rock, wherein the clay stone plays a role of thickening and suspending, preventing the phosphate rock and potassium-rich rock from partially sinking to the bottom during the hydrothermal reaction due to their high density, thereby reducing the contact area with water and affecting the extraction rate of phosphorus and potassium; the surfactant plays a role of fully wetting the surface of the ore in water, which is beneficial to the hydrothermal reaction and improves the extraction rate of phosphorus and potassium. DETAILED DESCRIPTION

[0016] In order to better understand the above technical solution, the technical solution of the present invention is described in detail below in conjunction with preferred examples. Example 1

[0017] A nanometer silicon-rich ore powder is prepared by grinding 50 parts of kaolinite, 25 parts of illite, 12 parts of phosphate rock and 42 parts of potassium feldspar and subjecting them to a hydrothermal reaction.

[0018] The hydrothermal reaction temperature is 220° C., the pressure is 0.5 MPa, and the pH is 8.5.

[0019] The preparation method of nano silicon-rich ore powder is carried out according to the following steps: S1. Initial stage of crushing treatment: put kaolinite, illite, phosphate rock and potassium feldspar into ore crusher and crush them into 15-20 mesh, mix them evenly, and obtain silicon-rich ore powder A; S2, further grinding and crushing the silicon-rich ore powder A to 170-200 mesh to obtain silicon-rich ore powder B; S3, adding water and sodium lignin sulfonate to the silicon-rich mineral powder B, stirring evenly, and then transferring to a sand mill to grind the mineral powder to a fineness of 2 to 20 microns, which is recorded as silicon-rich mineral dispersion C; S4, transfer the silicon-rich mineral dispersion C into a reactor, add 2 times of water, and perform hydrothermal reaction at a temperature of 220°C and a pressure of 0.5MPa for 20 hours to obtain a slurry, blow out the slurry through an air flow while it is hot, collect and cool it, and obtain fluffy silicon-rich ore powder; S5. The fluffy silicon-rich ore powder is crushed by a jet mill to obtain a two-dimensional mineral silicon flake material with a fineness of 17 to 56 nanometers, namely, nano silicon-rich ore powder.

[0020] In step S3, the mass ratio of silicon-rich ore powder B: water: sodium lignin sulfonate is 100:32:0.5.

[0021] Application of nano silicon-rich mineral powder: fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder as soil conditioner, directly applied to the soil; or The fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a fertilizer additive and applied to fertilizers. Example 2

[0022] A nanometer silicon-rich ore powder is prepared by grinding 55 parts of kaolinite, 22 parts of illite, 15 parts of phosphate rock and 43 parts of potassium feldspar and subjecting them to a hydrothermal reaction.

[0023] The hydrothermal reaction temperature is 200° C., the pressure is 0.6 MPa, and the pH is 9.0.

[0024] The preparation method of nano silicon-rich ore powder is carried out according to the following steps: S1. Initial stage of crushing treatment: put kaolinite, illite, phosphate rock and potassium feldspar into ore crusher and crush them into 15-20 mesh, mix them evenly, and obtain silicon-rich ore powder A; S2, further grinding and crushing the silicon-rich ore powder A to 170-200 mesh to obtain silicon-rich ore powder B; S3, adding water, sodium lignin sulfonate and alkylphenol polyoxyethylene ether to the silicon-rich mineral powder B, stirring evenly, and then grinding in a sand mill until the mineral powder fineness is 2 to 20 microns, which is recorded as silicon-rich mineral dispersion C; S4, transfer the silicon-rich mineral dispersion C into a reactor, add 1.5 times of water, and perform hydrothermal reaction at a temperature of 210°C and a pressure of 0.6MPa for 22 hours to obtain a slurry, blow out the slurry through an air flow while it is hot, collect and cool it, and obtain fluffy silicon-rich mineral powder; S5. The fluffy silicon-rich ore powder is crushed by a jet mill to obtain a two-dimensional mineral silicon flake material with a fineness of 17 to 56 nanometers, namely, nano silicon-rich ore powder.

[0025] In step S3, the mass ratio of silicon-rich mineral powder B: water: sodium lignin sulfonate: alkylphenol polyoxyethylene ether is 100:35:0.2:0.4.

[0026] Application of nano silicon-rich mineral powder: fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder as soil conditioner, directly applied to the soil; or Fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a fertilizer additive in fertilizers. Example 3

[0027] A nanometer silicon-rich ore powder is prepared by grinding 54 parts of kaolinite, 24 parts of illite, 14 parts of phosphate rock and 44 parts of potassium feldspar and subjecting them to a hydrothermal reaction.

[0028] The hydrothermal reaction temperature is 240° C., the pressure is 0.4 MPa, and the pH is 8.0.

[0029] The preparation method of nano silicon-rich ore powder is carried out according to the following steps: S1. Initial stage of crushing treatment: put kaolinite, illite, phosphate rock and potassium feldspar into ore crusher and crush them into 15-20 mesh, mix them evenly, and obtain silicon-rich ore powder A; S2, further grinding and crushing the silicon-rich ore powder A to 170-200 mesh to obtain silicon-rich ore powder B; S3, adding water, sodium naphthalenesulfonate and sodium polyacrylate to the silicon-rich mineral powder B, stirring evenly, and then grinding in a sand mill until the mineral powder fineness is 2 to 20 microns, which is recorded as silicon-rich mineral dispersion C; S4, transfer the silicon-rich mineral dispersion C into a reactor, add 2 times of water, and perform hydrothermal reaction at a temperature of 240°C and a pressure of 0.5MPa for 18 hours to obtain a slurry, blow out the slurry through an air flow while it is hot, collect and cool it, and obtain fluffy silicon-rich mineral powder; S5. The fluffy silicon-rich ore powder is crushed by a jet mill to obtain a two-dimensional mineral silicon flake material with a fineness of 17 to 56 nanometers, namely, nano silicon-rich ore powder.

[0030] In step S3, the mass ratio of silicon-rich ore powder B: water: sodium naphthalenesulfonate: sodium polyacrylate is 100:38:0.1:0.8.

[0031] Application of nano silicon-rich mineral powder: fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder as soil conditioner, directly applied to the soil; or Fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a fertilizer additive in fertilizers. Example 4

[0032] A nanometer silicon-rich ore powder is prepared by grinding 60 parts of kaolinite, 22 parts of illite, 15 parts of phosphate rock and 55 parts of potassium feldspar and subjecting them to a hydrothermal reaction.

[0033] The hydrothermal reaction temperature is 250° C., the pressure is 0.5 MPa, and the pH is 8.5.

[0034] The preparation method of nano silicon-rich ore powder is carried out according to the following steps: S1. Initial stage of crushing treatment: put kaolinite, illite, phosphate rock and potassium feldspar into ore crusher and crush them into 15-20 mesh, mix them evenly, and obtain silicon-rich ore powder A; S2, further grinding and crushing the silicon-rich ore powder A to 170-200 mesh to obtain silicon-rich ore powder B; S3, adding water and sodium polyacrylate to the silicon-rich mineral powder B, stirring evenly, and then grinding in a sand mill until the mineral powder fineness is 2 to 20 microns, which is recorded as silicon-rich mineral dispersion C; S4, transfer the silicon-rich mineral dispersion C into a reactor, add 2 times of water, and perform hydrothermal reaction at a temperature of 240°C and a pressure of 0.6MPa for 24 hours to obtain a slurry, blow out the slurry through an air flow while it is hot, collect and cool it, and obtain fluffy silicon-rich mineral powder; S5. The fluffy silicon-rich ore powder is crushed by a jet mill to obtain a two-dimensional mineral silicon flake material with a fineness of 17 to 56 nanometers, namely, nano silicon-rich ore powder.

[0035] In step S3, the mass ratio of silicon-rich ore powder B: water: sodium polyacrylate is 100:40:1.

[0036] Apply fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder directly to the soil as a soil conditioner; or The fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a fertilizer additive and applied to fertilizers.

[0037] The beneficial effects of the present invention are further illustrated below in conjunction with test data: Experiment 1 1.1 Experimental location: Ban Lao Shi Special Fertilizer Research and Design Institute (Henan) Co., Ltd.

[0038] 1.2 Experimental detection: thickness (nm), K2O (%), P2O5 (%) and SiO2 (%), and calculate the extraction rate.

[0039] 1.3 Test samples: Comparison 1 (except that kaolinite and illite were not added, the rest were consistent with Example 1), Comparison 2 (except that illite was reduced by 15 parts and potassium feldspar was increased by 15 parts, i.e., 50 parts of kaolinite, 10 parts of illite, 12 parts of phosphate rock and 57 parts of potassium feldspar, the rest were consistent with Example 1), Comparison 3 (except that kaolinite was reduced by 15 parts and potassium feldspar was increased by 15 parts, i.e., 35 parts of kaolinite, 25 parts of illite, 12 parts of phosphate rock and 57 parts of potassium feldspar, the rest were consistent with Example 1), Comparison 4 (except that sodium lignin sulfonate was not added, the rest were consistent with Example 1) and the nano silicon-rich ore powder prepared in Example 1.

[0040] 1.4 Detection method: Use atomic force microscopy to detect thickness; K2O (%), P2O5 (%) and SiO2 (%) detection: 1. Preparation of test solution: Place the sample in a dry 250mL volumetric flask, add 150mL of 20g / L citric acid solution pre-heated to 28-30℃, and seal the bottle mouth tightly. Keep the solution temperature between 28 and 30°C, oscillate on an oscillator for 1 hour, take out the volumetric flask, make up to volume with water and shake well, dry filter, discard the initial filtrate, and the filtrate obtained is the test solution. If the K2O content is greater than 10%, weigh 1g, and if the K2O content is less than 10%, weigh 2g. 2. Detection: respectively aspirate 15ml of the test solution, detect K2O (%) and P2O5 (%), use the potassium tetraphenylborate weight method for potassium oxide detection, and use the quinolyphosate weight method for phosphorus pentoxide detection; for silica detection, aspirate 15ml of the test solution, add water to 40ml, add 10ml of nitric acid, and detect according to the determination method of water-soluble silica in fertilizers.

[0041] The phosphorus pentoxide actually detected by this method is the sum of water-soluble phosphorus and citrate-soluble phosphorus, and the potassium detected is equivalent to the sum of citrate-soluble potassium and water-soluble potassium; the silicon dioxide is the sum of citrate-soluble silicon dioxide and water-soluble silicon, because the citrate-soluble and water-soluble substances in fertilizers are considered to be absorbable by plants.

[0042] Except for the experimental treatment, other operations were the same in this experiment.

[0043] The content of the mixed ore in comparison 1 is P2O5 6.7%, K2O 13.0%, SiO2 51.2%; The content of components in the mixed ore of comparison 2 is P2O5 2.8%, K2O 7.7%, SiO2 49.5%; The content of the mixed ore in comparison 3 is P2O5 2.8%, K2O 8.4%, SiO2 49.6% The contents of the components in the mixed ore of comparison 4 are P2O5 2.8%, K2O 6.1%, and SiO2 47.2%; The content of components in the mixed ore of Example 1 is P2O5 2.8%, K2O 6.2%, SiO2 47.4%; The mineral powder adopts the ore testing method, which is a full analysis and is dissolved in nitric acid. Therefore, many ingredients cannot be absorbed by plants.

[0044] 2 Results and analysis Thickness (nm), K2O (%), P2O5 (%) and SiO2 (%), test data are shown in Table 1

[0045] Among them, the extraction rate of K2O in comparison 1 is 17.8%; the extraction rate of P2O5 is 17.9%; the extraction rate of SiO2 is 18.0%; In comparison 2, the extraction rate of K2O is 27.3%; the extraction rate of P2O5 is 21.4%; and the extraction rate of SiO2 is 23.6%; In comparison 3, the extraction rate of K2O is 27.4%; the extraction rate of P2O5 is 21.4%; and the extraction rate of SiO2 is 24.0%; In comparison 4, the extraction rate of K2O is 29.5%; the extraction rate of P2O5 is 25%; and the extraction rate of SiO2 is 30.3%; In Example 1, the extraction rate of K2O is 32.3%; the extraction rate of P2O5 is 28.6%; and the extraction rate of SiO2 is 31.0%.

[0046] From the comparison of the data of Comparison 1, Comparison 2, Comparison 3 and Example 1, it can be seen that the addition of clay can improve the extraction rate of K2O (%), P2O5 (%) and SiO2 (%). It may be that the clay plays an anti-precipitation role, increases the contact area between the ore and water, and thus improves the extraction rate; further, in Example 1, where the total mass fraction of clay is greater than the total mass fraction of phosphate ore and potassium-rich rock, its K2O (%), P2O5 (%) and SiO2 (%) extraction rates are also significantly higher than those of Comparison 2 and Comparison 3, where the total mass fraction of clay is less than the total mass fraction of phosphate ore and potassium-rich rock. It can be seen that the total mass fraction of clay and the total mass fraction of phosphate ore and potassium-rich rock also affect the extraction rates of K2O (%), P2O5 (%) and SiO2 (%).

[0047] From the comparison of the data of Comparative 4 and Example 1, it can be seen that the addition of surfactant also affects the extraction rate of K2O (%), P2O5 (%) and SiO2 (%), and Example 1 has the best extraction effect.

[0048] Experiment 2 1.1 Test location: Shuangcheng District, Harbin City, Heilongjiang Province, paddy field, rice variety is Longdao No. 22.

[0049] 1.2 Experimental tests: soil EC1:5 (ds / m3) before transplanting, soil EC1:5 (ds / m3) after harvesting, pH before transplanting and after harvesting, sheath blight rate (%), tillering per plant (pieces / plant), 1000-grain weight (g), and yield (kg / mu).

[0050] 1.3 Test samples: Comparison 1 (except that kaolinite and illite were not added, the rest were consistent with Example 1), Comparison 2 (except that illite was reduced by 15 parts and potassium feldspar was increased by 15 parts, i.e., 50 parts of kaolinite, 10 parts of illite, 12 parts of phosphate rock and 57 parts of potassium feldspar, the rest were consistent with Example 1), Comparison 3 (except that kaolinite was reduced by 15 parts and potassium feldspar was increased by 15 parts, i.e., 35 parts of kaolinite, 25 parts of illite, 12 parts of phosphate rock and 57 parts of potassium feldspar, the rest were consistent with Example 1), Comparison 4 (except that sodium lignin sulfonate was not added, the rest were consistent with Example 1) and 20 kg each of the nano silicon-rich ore powder prepared in Example 1.

[0051] 1.4 Test method: 28-5-5 nitro controlled-release fertilizer was selected as base fertilizer, and 5 mu of rice field was divided into 5 plots, corresponding to Comparison 1 (except that kaolinite and illite were not added, the others were consistent with Example 1), Comparison 2 (except that illite was reduced by 15 parts and potassium feldspar was increased by 15 parts, i.e., kaolinite was 50 parts, illite was 10 parts, phosphate rock was 12 parts and potassium feldspar was 57 parts, the others were consistent with Example 1), Comparison 3 (except that kaolinite was reduced by 15 parts and potassium feldspar was increased by 15 parts, i.e., kaolinite was 35 parts, illite was 25 parts, phosphate rock was 12 parts and potassium feldspar was 57 parts, the others were consistent with Example 1), Comparison 4 (except that sodium lignin sulfonate was not added, the others were consistent with Example 1) and Example 1, nano silicon-rich ore powder and base fertilizer were applied together, the amount of nano silicon-rich ore powder was 20 kg / plot, and the amount of base fertilizer was 40 kg / plot.

[0052] 2. Results Soil EC1:5 (ds / m3) before transplanting, soil EC1:5 (ds / m3) after harvest, pH before transplanting and after harvest, sheath blight rate (%), tillering per plant (unit / plant), 1000-grain weight (g), and yield (kg / mu) are shown in Table 2

[0053] From the above data in combination with Table 1 and Table 2, it can be seen that from the comparison of the data of Comparison 1, Comparison 2, Comparison 3 and Example 1, it can be seen that the addition of clay can not only improve the extraction rate of K2O (%), P2O5 (%) and SiO2 (%), but also better improve the soil and increase crop yields; further, Example 1 in which the total mass fraction of clay is greater than the total mass fraction of phosphate ore and potassium-rich rock is significantly higher than Comparison 2 and Comparison 3 in which the total mass fraction of clay is less than the total mass fraction of phosphate ore and potassium-rich rock in terms of improving soil and increasing crop yields. It can be seen that the total mass fraction of clay and the total mass fraction of phosphate ore and potassium-rich rock also affect soil improvement and crop yields.

[0054] From the comparison of the data between Comparative Example 4 and Example 1, it can be seen that the addition of surfactant not only affects the extraction rate of K2O (%), P2O5 (%) and SiO2 (%), but also affects the improvement of the soil and the increase of crop yield by the product. Example 1 prepared in this application has the best effect.

[0055] Since the present application can improve the soil, thereby improving the disease resistance of crops, the present application is significantly superior to the comparative example in preventing sheath blight.

Claims

1. A nano silicon-rich ore powder, It is characterized in that The method is prepared by grinding clay stone, phosphate rock and potassium-rich rock and subjecting them to hydrothermal reaction; and the mass fraction of the clay stone is greater than the total mass fraction of the phosphate rock and the potassium-rich rock.

2. The nano silicon-rich ore powder as claimed in claim 1, It is characterized in that The clay stone is one or both of kaolinite and illite; the potassium-rich rock is one or both of mica and potassium feldspar.

3. The nano silicon-rich ore powder as claimed in claim 1 or 2, It is characterized in that 50-60 parts of kaolinite, 10-15 parts of phosphate rock, 20-30 parts of illite, and 40-60 parts of potassium-rich rock, and the total mass fraction of kaolinite and illite is greater than the total mass fraction of phosphate rock and potassium-rich rock.

4. The nano silicon-rich ore powder as claimed in claim 1, It is characterized in that The hydrothermal reaction temperature is 165-255° C., the pressure is 0.4-0.6 MPa, and the pH is 8.0-10.

5. The method for preparing the nano silicon-rich ore powder according to any one of claims 1 to 4, It is characterized in that Follow these steps: S1. Initial stage of crushing: put the clay stone, phosphate rock and potassium-rich rock into the ore crusher and crush them into 15-20 mesh, mix them evenly, and obtain silicon-rich ore powder A; S2, further grinding and crushing the silicon-rich ore powder A to 170-200 mesh to obtain silicon-rich ore powder B; S3, adding water and surfactant to the silicon-rich mineral powder B, stirring evenly, and then grinding in a sand mill until the mineral powder fineness is 2 to 20 microns, which is recorded as silicon-rich mineral dispersion C; S4, transfer the silicon-rich mineral dispersion C into a reactor, add 1 to 3 times of water, and perform hydrothermal reaction at a temperature of 165 to 255°C and a pressure of 0.4 to 0.6 MPa for 16 to 24 hours to obtain a slurry, blow out the slurry while it is hot through an air flow, collect and cool it, and obtain fluffy silicon-rich mineral powder; S5. The fluffy silicon-rich ore powder is crushed by a jet mill to obtain a two-dimensional mineral silicon flake material with a fineness of 17 to 56 nanometers, namely, nano silicon-rich ore powder.

6. The method for preparing the nano silicon-rich ore powder according to claim 5, It is characterized in that The surfactant is one or a mixture of two or more of sodium hexametaphosphate, sodium pyrophosphate, sodium polyacrylate, triethanolamine, sodium lignin sulfonate, sodium naphthalene sulfonate and alkylphenol polyoxyethylene ether.

7. The method for preparing the nano silicon-rich ore powder according to claim 5, It is characterized in that In step S3, the mass ratio of silicon-rich ore powder B: water: surfactant is 100:30-40:0.2-2.

8. Application of the nano silicon-rich ore powder according to any one of claims 1 to 7, It is characterized in that The fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a soil conditioner and directly applied to the soil; or the fluffy silicon-rich mineral powder and / or nano silicon-rich mineral powder is used as a fertilizer additive and applied to fertilizer.

Citation Information

Patent Citations

  • Method for producing phosphorus-potassium-silicone-calcium multi-element microporous mineral fertilizer (soil conditioner)

    CN104844302A

  • PRE-FERTILIZER INPUT, PROCESS FOR OBTAINING A BROAD-SPECTRUM MULTINUTRIENT FERTILIZER COMPOSITION AND FERTILIZING, REMINERALIZING AND PHYTOPROTECTIVE COMPOSITIONS