Polyol N-8OH and preparation method thereof, and glycidyl ether type epoxy resin and preparation method thereof

Extract polyol N-8OH from epoxy resin through alcoholysis technology and prepare glycidyl ether type epoxy resin, which solves the problem of difficulty in recycling and reusing traditional epoxy resin and realizes low-cost recycling and reuse of epoxy resin. High performance reuse for a variety of high heat resistant applications.

CN118724732APending Publication Date: 2024-10-01SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410711706.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Due to its high cross-linking density and covalent cross-linking structure, traditional epoxy resin is difficult to recycle and reuse, and its thermal stability and degradability are inconsistent, resulting in environmental pollution problems in applications in low-temperature fields.

Method used

Extract polyol N-8OH from epoxy resin through alcoholysis technology, and use it with epichlorohydrin and other raw materials to prepare glycidyl ether type epoxy resin to realize the recovery and reuse of epoxy resin, using ethylene glycol Alcohol degradation and purification processes, combined with the use of anhydrides or amine curing agents, ensure the cleavage and resynthesis of ester bonds.

Benefits of technology

It achieves low-cost recycling and reuse of epoxy resin, reduces process energy consumption, and produces glycidyl ether type epoxy resin with better flexibility and heat resistance, suitable for high heat resistance and low viscosity application scenarios. , such as electronic packaging and wind turbine blades.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724732A_ABST
    Figure CN118724732A_ABST
Patent Text Reader

Abstract

The invention provides a polyol N-8OH with a structural formula as shown in a formula I: # imgabs0 #. The invention also provides a preparation method of the polyol N-8OH, and a glycidyl ether type epoxy resin and a preparation method thereof. The polyhydric alcohol comes from the waste epoxy cured product, the raw material cost is low, the added value of the product obtained after recovery and conversion is high, the energy consumption in the recovery process is low, and the method is green and environment-friendly. The prepared glycidyl ether type epoxy resin is nitrogen-containing alicyclic polyepoxy functional group resin and is mainly used as an adhesive. Compared with common epoxy (bisphenol A epoxy containing benzene ring), the epoxy resin has better flexibility and lower viscosity; compared with aliphatic epoxy without a cyclic structure, the aliphatic epoxy resin has higher heat resistance and is more suitable for scenes requiring high heat resistance and low viscosity, such as electronic packaging resin, vacuum infusion resin for wind power blades and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyol N-8OH and a preparation method thereof, and a glycidyl ether type epoxy resin and a preparation method thereof. Background Art

[0002] In recent years, thermosetting epoxy resins are an important component of high-performance resins. Due to their excellent thermal, mechanical and insulation properties and processability, they play an important role in many fields of polymer materials. Such as coatings, adhesives and composite substrate materials. In the field of low temperature, epoxy resins can be used as adhesives, insulating materials and composite materials, coils, resin matrices of large superconducting magnets and other important equipment. However, due to their high cross-linking density, traditional epoxy resins cannot be modified, repaired or recycled. Therefore, waste materials such as wind blades and vehicles are usually landfilled or pyrolyzed, causing environmental pollution. For the sake of resources and the environment, the recycling of epoxy resins by chemical solvents has gradually emerged. However, due to their three-dimensional covalent cross-linking network, traditional epoxy resins are also severely limited in chemical recycling. At the same time, due to the similarity of their covalent cross-linking structures, it is still a challenge to separate the mixed degradation products to achieve the purpose of reuse of each component.

[0003] Ester groups are one of the most commonly used functional groups in recyclable epoxy systems because they can be cleaved under acidic, neutral or alkaline conditions. Typically, such ester-based thermosetting epoxy resins are obtained by the reaction between epoxy precursors and anhydrides or carboxylic acids. Ester-based thermosetting epoxy resins containing primary hydroxyl groups have high thermal stability and usually require chemical treatment to break off. Hydrolysis, alcoholysis and aminolysis are more mature methods, but they usually require harsh conditions. Although the decomposition of ester-based epoxy resins is highly controllable, they are not commonly used in industry because they are susceptible to moisture and catalysts, which hinder their long-term stability. In addition, their high Tg is inconsistent with degradability. At the same time, for all ester-based thermosetting epoxy resins, the depolymerization products are a mixture of oligomers and cannot be effectively separated. Therefore, it is challenging to develop a closed-loop recycling strategy aimed at continuously preparing almost identical epoxy resin systems.

[0004] Alcoholysis refers to the dissolution of the epoxy matrix by catalyzing the transesterification reaction between the ester groups of the epoxy polymer and the added alcohol. In addition, alcoholysis can be carried out with liquids or critical fluids. Supercritical or near-critical fluids are able to degrade the epoxy resin network in an irregular manner. The liquids generally used for alcoholysis are simple alcohols such as methanol, ethanol and propanol. Shi0 et al. developed epoxy resins based on bisphenol A diglycidyl ether (DGEBA), fatty acid mixtures and glutaric anhydride (GA) hardener. The Tg of the prepared epoxy resin increases with the reduction of the fatty acid content in the formulation. In addition, the epoxy resin was soaked in 2-ethyl-1-hexanol and ethylene glycol alcohol solvents at 160°C and triazacyclo[4.4.0]dodec-5-ene (TBD) transesterification catalyst to study the transesterification reaction of the network. The results showed that the dissolution rate of the resin increased with the increase of the anhydride curing agent ratio in the epoxy system due to the high mobility of the shorter chain segments.

[0005] In another study, DGEBA-based epoxy resin cured with 1,2-cyclohexanedicarboxylic anhydride (CHCA) was effectively depolymerized by supercritical methanolysis. The depolymerized solution contained hydroxyl and ester functional groups, and a new thermosetting resin was prepared using the same curing agent under triethylamine catalysis, which can be used as a substitute for bisphenol-based thermosetting epoxy resin. Although effective reuse of the resin was achieved, the mechanical properties were reduced, with the tensile strength of the original epoxy material being 100 MPa, while the tensile strength of the recycled resin was about 70 MPa0 due to the lower crosslinking density.

[0006] Application number: CN202211507989.6, invention name: A recyclable epoxy resin and its preparation method and recycling method, which relates to a recyclable epoxy resin and its preparation method and recycling method. The recyclable epoxy resin of the present invention comprises, in terms of mass percentage: 45% to 65% epoxy resin raw material, 35% to 55% curing agent and 0.05% to 5% catalyst. The specific preparation process includes: heating and mixing the above components evenly, degassing under vacuum, and then curing to obtain a recyclable epoxy resin with recycling performance. This patent uses a hyperbranched polyether epoxy resin, and the ester bond that can be broken by ethylene glycol is introduced from the curing agent anhydride; however, if an amine curing agent is used, there is no ester bond inside the system, and it cannot be degraded by ethylene glycol. Summary of the invention

[0007] The technical solution of the present invention is to provide a polyol N-8OH and a preparation method thereof, as well as a glycidyl ether type epoxy resin and a preparation method thereof. The polyol N-8OH is a recovered product of the epoxy resin, and the polyol N-8OH is recycled.

[0008] The present invention provides a polyol N-8OH, the structural formula of which is shown in Formula I:

[0009]

[0010] It is extracted and separated from the alcoholysis product of thermosetting epoxy resin.

[0011] Furthermore, the cured epoxy resin is degraded by using ethylene glycol, and the obtained degradation liquid is purified to obtain the polyol N-8OH.

[0012] The process route is:

[0013] The specific steps include:

[0014] a. Curing of epoxy resin:

[0015] TDTMSE is used as a monomer and IPDA is used as a curing agent. The two are mixed evenly at room temperature, poured into a mold coated with a silicone release agent, and then vacuum degassed. After the bubbles are removed, the epoxy resin (EP) is cured according to a thermal curing procedure of 80°C / 6h; wherein the mass ratio of the curing agent amount to the monomer amount is 25.5:100;

[0016] b. Degradation of epoxy resin:

[0017] EP:ethylene glycol (EG) in a mass ratio of 1:9 was added into a three-necked flask equipped with a condenser, a stirring device, and a heating device, and nitrogen was introduced to exhaust the air in the device, and then the temperature was raised to 180°C for degradation for 3 hours to obtain EP alcoholysis solution (GEP);

[0018] c. Purification of polyol N-8OH:

[0019] Remove EG from the alcoholysis solution of EP in step b to obtain a viscous brown mixed solution (DEP); add NaOH for alkaline hydrolysis, the mass of NaOH is 20% of the total mass of DEP, and a 5% NaOH solution is prepared and added to the flask, and the temperature is raised to 60°C for reaction for 2.5 hours. After the reaction is completed, distill off water to obtain a viscous brown mixed solution (NEP);

[0020] Add anhydrous ethanol to NEP, let stand for 24 hours, filter, take the filtrate and add hydrochloric acid to adjust the pH of the clear liquid to neutral, and obtain a yellow clear filtrate. The filtrate is subjected to rotary evaporation at 80°C to completely remove the ethanol, and a viscous dark red liquid (HEP) is obtained;

[0021] The residual EG in HEP ​​was extracted by a solvent method to obtain N-8OH, wherein the solvents were ethyl acetate (EAC) and acetone (AC), and the volume ratio of acetone to ethyl acetate was 1:15.

[0022] The present invention also provides application of the preparation method of the polyol N-8OH in a method for recovering epoxy resin.

[0023] The present invention provides a glycidyl ether type epoxy resin EP / N-8OH, which is prepared from the polyol N-8OH, and has the structural formula:

[0024]

[0025] The glycidyl ether epoxy resin EP / N-8OH is prepared using polyol N-8OH and epichlorohydrin (ECH) as raw materials and boron trifluoride ethyl ether (BF3·OEt2) as a catalyst, wherein the molar ratio of polyol N-8OH to epichlorohydrin (ECH) is 1:2.1-2.3.

[0026] Furthermore, it is prepared from the polyol N-8OH and epichlorohydrin (ECH) as raw materials described in claim 1, and boron trifluoride ethyl ether (BF3·OEt2) as a catalyst, and undergoes ring-opening etherification and alkali-adding ring-closing reaction to obtain a glycidyl ether type epoxy resin EP / N-8OH; the molar ratio of N-8OH to ECH is 1:2.2; and the amount of boron trifluoride ethyl ether (BF3·OEt2) used is 0.5% of the mass of N-8OH.

[0027] The process route is:

[0028]

[0029] Specifically, the steps include:

[0030] a. Take N-8OH and ECH in a molar ratio of 1:(2.1-2.3), heat to 50-80°C, add BF3·Et2O with a catalyst mass of 0.3-0.7% of the mass of N-8OH, heat to 80°C and react for 1-5h to perform etherification ring opening;

[0031] b. After cooling to 55°C, add 12.5wt% NaOH aqueous solution and react for 2h;

[0032] c. After the ring closure is completed, dichloroethane (DCE) and distilled water are added to wash until the lower liquid is neutral, and the lower organic phase is retained by separation to obtain a uniform degradation product of the epoxy resin; the ECH and DCE solvents are removed by rotary evaporation to obtain an orange-red viscous liquid, i.e., a new epoxy resin prepolymer EP / N-8OH synthesized from nitrogen-containing polyols;

[0033] d. Curing: Use EP / N-8OH as monomer and IPDA as curing agent, mix the two thoroughly at room temperature, pour into a mold coated with silicone release agent, and then perform vacuum degassing until there are no bubbles. Complete the curing of EP / N-8OH according to the curing procedure of 80℃ / 6h.

[0034] Among them, the step a is: take N-8OH and ECH with a molar ratio of 1:2.2, heat to 50°C, add BF3·Et2O with a catalyst mass of 0.5% of the mass of N-8OH, heat to 65°C for reaction for 1h, and perform etherification ring opening; the curing conditions described in step d are: the amount of IPDA is 18.34% of the mass of EP / N-8OH; and cure at 80°C / 6h.

[0035] The glycidyl ether epoxy resin prepared by the present invention is a nitrogen-containing aliphatic ring type polyepoxy functional group resin, and its main use is adhesive. It can be used for flame retardant epoxy (it contains nitrogen and can form NP synergy with P and Si flame retardants, or N-Si synergy, without the need to add an additional N source, such as ammonium polyphosphate, etc.); because it contains aliphatic rings, it has better flexibility and lower viscosity than ordinary epoxy (bisphenol A type epoxy, containing benzene rings); and compared with aliphatic epoxies without cyclic structures, it has higher heat resistance and is more suitable for scenes requiring high heat resistance and low viscosity: such as electronic packaging resins, vacuum infusion resins for wind turbine blades, etc.

[0036] The epoxy molecules of the present invention contain ester bonds inside, and can be degraded by alcoholysis with ethylene glycol regardless of whether an amine curing agent or an acid anhydride curing agent is used; the nitrogen-containing polyol structure of the present invention can only be obtained by using an epoxy containing an ester bond and an amine curing agent at the same time. The present invention can dissolve the solidified recyclable epoxy resin in a composite solvent under heating conditions, and then recover the composite solvent by vacuum distillation, and can recover and reuse the low-molecular polyol obtained by dissolution and degradation. The polyol of the present invention is derived from waste epoxy cured products, and the raw material cost is low. The products obtained after recovery and conversion have high added value, and the recovery process has low energy consumption and is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of alcoholysis of epoxy resin;

[0038] Figure 2 Epoxy resin EP / N-8OH synthesized from polyols

[0039] Figure 3 Schematic diagram of N-8OH epoxidation reaction

[0040] Figure 4 Effect of different V(EAC) / V(AC) on HEP ​​hydroxyl value

[0041] Figure 5 The purified N-8OH NMR hydrogen spectrum

[0042] Figure 6 H NMR spectrum of EP / N-8OH

[0043] Figure 7DEP infrared spectra of epoxy resin and alcoholysis solution

[0044] Figure 8 Infrared spectrum of N-8OH refining process

[0045] Fig. 9 Infrared spectra of N-8OH and EP / N-8OH

[0046] Fig.10 Chromatogram of epoxy resin alcoholysis solution DEP

[0047] Fig.11 Mass spectrum of epoxy resin alcoholysis solution with DEP retention time of 0.6min

[0048] Fig.12 Thermal properties of EP and EP / N-8OH cured samples

[0049] Fig.13 Impact and flexural strength graphs of EP and EP / N-8OH cured specimens

[0050] Fig.14 Stress-strain curves of EP and EP / N-8OH cured samples DETAILED DESCRIPTION

[0051] Example 1 Extraction of polyol monomers of the present invention

[0052] 2.2.1 Curing of epoxy resin

[0053] TDTMSE is used as a monomer and IPDA is used as a curing agent (the amount of curing agent: the amount of monomer = 25.5:100). The two are mixed evenly at room temperature and poured into a mold coated with a silicone release agent, and then vacuum degassed. After the bubbles are removed, the epoxy resin (EP) is cured according to the 80℃ / 6h thermal curing procedure. The EP cured sample strips are cut into fine powder by a crusher.

[0054] The amount of curing agent and monomer is calculated based on the complete reaction formula between epoxy resin and amine curing agent. The specific formula is:

[0055] The amount of amine that needs to be added to 100g of epoxy resin = epoxy value of epoxy resin × (molecular weight of amine curing agent / number of active hydrogens in amine curing agent).

[0056] The epoxy value of the epoxy resin is measured to be 0.6, the molecular weight of the curing agent IPDA is 170.29, and the number of active hydrogens is 4. Therefore, the amount of 100g of epoxy resin IPDA is 0.6×(170.29 / 4)=25.5.

[0057] 2.2.2 Degradation of epoxy resin

[0058] EP:ethylene glycol (EG) at a mass ratio of 1:9 was added into a three-necked flask equipped with a condenser, a stirring device and a heating device. After nitrogen was introduced to exhaust the air in the device, the temperature was raised to 180°C for degradation for 3 hours to obtain the alcoholysis solution (GEP) of EP.

[0059] 2.2.3 Extraction of polyol monomers

[0060] GEP is further purified to obtain polyol (N-8OH). The extraction of N-8OH from the alcoholysis solution is divided into three steps:

[0061] (1) GEP is subjected to vacuum distillation to remove EG to obtain a viscous brown mixed solution (DEP), which is then alkaline hydrolyzed by adding NaOH, wherein the mass of NaOH is 20% of the total mass of DEP. A 5% NaOH solution is prepared and added to a flask. The temperature is raised to 60°C and the reaction is carried out for 2.5 hours. After the reaction is completed, water is distilled off to obtain a viscous brown mixed solution (NEP).

[0062] (2) Anhydrous ethanol was added to NEP, and the mixture was allowed to stand for 24 h. The mixture was filtered and the filtrate was taken and hydrochloric acid was added to adjust the pH of the clear solution to neutral to obtain a yellow clear filtrate. The filtrate was subjected to rotary evaporation at 80°C to completely remove the ethanol and obtain a viscous dark red liquid (HEP).

[0063] (3) The optimal volume ratio of ethyl acetate (EAC): acetone (AC) is 1:15. The residual EG in HEP ​​is extracted by solvent method. The hydroxyl value of the solution after EG is extracted from HEP is determined by dianhydride-pyridine method. The optimal compounding ratio is selected to extract the residual EG in HEP ​​to obtain the final product, which is high-purity N-8OH.

[0064] The process route is:

[0065]

[0066] Component analysis of epoxy resin alcoholysis solution DEP:

[0067] EG is used to carry out alcoholysis and depolymerization of epoxy resin. The alcoholysis structure diagram is shown in Figure 1 As shown in (a). According to the special structure of the ester bond contained in TDTMSE, the cured EP is added to the EG solution at a certain temperature. In the absence of a catalyst, EG acts as a high boiling point solvent, and the hydroxyl part attacks the ester bond part in the epoxy resin, and an ester exchange reaction occurs. The cross-linked network structure of the cured EP is destroyed and finally degraded into oligomers. The ester EP achieves rapid degradation in a short time, and the recovered degradation liquid GEP is obtained. By Figure 1(b) It can be seen that after degradation, the epoxy functional group of EP is transformed into a terminal dihydroxy structure, and an octahydric alcohol structure is generated with the IPDA curing part, and the hydroxyl group contained in the degradation system increases. At the same time, the oligomers produced after depolymerization and bond breaking are easily separated by vacuum distillation, and the residual high boiling point solvent EG can be removed by rotary evaporation to obtain the alcoholysis solution DEP, and its components are further analyzed.

[0068] Example 2 Synthesis of a novel epoxy resin (EP / N-8OH)

[0069] (1) Preparation of EP / N-8OH: Add N-8OH and ECH in a molar ratio of 1:2.2 to a three-necked flask equipped with a thermometer, a stirring device, and a reflux condenser, heat to 50°C, add dropwise BF3·Et2O in a catalyst mass of 0.5% of the mass of N-8OH, heat to 80°C and react for 1 hour to carry out etherification ring opening. After cooling to 55°C, add dropwise 12.5wt% NaOH aqueous solution and react for 2 hours. After the ring closure is completed, add dichloroethane (DCE) and distilled water to wash until the lower layer of liquid is neutral, separate the liquid and retain the lower organic phase to obtain a uniform degradation product of epoxy resin. Rotary evaporation is used to remove solvents such as ECH and DCE to obtain an orange-red viscous liquid, which is a new epoxy resin prepolymer EP / N-8OH synthesized from nitrogen-containing polyols (see Figure 2 ).

[0070] (2) Curing of EP / N-8OH epoxy resin: Based on the previous step, an orthogonal experiment was designed to optimize the etherification ring-opening process for synthesizing EP / N-8OH. Under the optimal etherification ring-opening process conditions and through a 55℃ / 2h closed-loop epoxidation procedure, EP / N-8OH with a high epoxy value was synthesized. EP / N-8OH was used as a monomer and IPDA as a curing agent. The two were thoroughly mixed at room temperature and poured into a mold coated with a silicone release agent. Then, vacuum degassing was performed until there were no bubbles. The EP / N-8OH was cured according to a curing procedure of 80℃ / 6h.

[0071] The synthesis diagram of the new epoxy resin (EP / N-8OH) synthesized with high-purity N-8OH as a monomer is as follows. The acidic catalyst boron trifluoride·ether complex was selected for epoxidation reaction. The reaction was carried out in two steps, the first step was etherification, and the second step was alkali ring closure. The synthesis principle is that in the first step, N-8OH forms a complex with the ether in BF3·Et2O to generate a positive and negative ion pair, and then reacts with ECH to generate an etherification intermediate, such as Figure 3 The second step is that the etherification intermediate removes the chlorine atoms at both ends under the action of NaOH to form the corresponding chloride, which is then subjected to a ring-closing reaction to generate EP / N-8OH.

[0072] Example 3 EP / N-8OH Synthesis Process Parameter Screening Test

[0073] On the basis of synthesizing EP / N-8OH, the experiment first explored the type of catalyst, and explored the effect of phase transfer catalysts tetrabutylammonium bromide and benzyltrimethylammonium chloride on the synthesis of EP / N-8OH. The experimental results showed that the epoxy value of the glycidyl ether EP / N-8OH synthesized by this type of phase transfer catalyst was low and the yield was small. Therefore, the experiment finally determined to use the acidic catalyst BF3·Et2O. Based on this catalyst and the original closed-loop procedure, the four main factors of the etherification synthesis process n(ECH) / n(N-8OH hydroxyl), catalyst dosage (mass fraction of N-8OH), etherification temperature and time were optimized. Three levels were selected for each factor, so the orthogonal table L9(3 4 ) Experiments were carried out, and the results and analysis are shown in Table 3-1.

[0074] Table 3-1 Orthogonal test design table

[0075]

[0076] Table 3-2 Orthogonal test results

[0077]

[0078] Table 3-3 Orthogonal test level analysis

[0079]

[0080] The structural reaction analysis of the optimized synthesized EP / N-8OH was carried out based on the epoxy value of the product. From the analysis results in the previous section, it can be seen that N-8OH contains 8 hydroxyl functional groups (M=466g / mol). If only one hydroxyl group (-OH) in the N-8OH structure loses hydrogen (M=1g / mol) to participate in the epoxidation reaction and is converted into an epoxy group (M=57g / mol), then the molecular weight increased by 56g / mol after the epoxidation of one hydroxyl group in the N-8OH structure. Therefore, the number of hydroxyl groups actually participating in the epoxidation reaction in N-8OH can be calculated according to formula (3-1).

[0081]

[0082] Where:

[0083] n is -OH participating in the epoxidation reaction

[0084] Le is the theoretical epoxy value after n hydroxyl groups participate in the reaction (mol / 100g)

[0085] The range analysis of the orthogonal test results shows that the amount of ECH has the greatest impact on the yield and epoxy value. At the same time, the optimal combinations A2B2C2D1 and A3B1C1D3 were determined through orthogonal tests. The properties of the epoxy resins synthesized by the two optimized combinations are given in Table 3-4 below. It can be seen from Table 3-4 that the epoxy value and yield of EP / N-8OH after A2B2C2D1 optimization are slightly higher. Therefore, A2B2C2D1 is the most suitable process condition within the selected process condition range, that is, the molar ratio of N-8OH to ECH is 1:2.2, the amount of catalyst BF3·OEt2 is 0.5% of the mass of N-8OH, and the etherification reaction program is 65℃ / 1h.

[0086] It is calculated from formula 3-1 that under the optimal synthesis conditions A2B2C2D1, the number of -OH groups actually participating in the epoxidation reaction in the N-8OH structure is 2.6. Therefore, according to the epoxy value of EP / N-8OH synthesized under this optimized process of 0.43 mol / 100 g, the amount of IPDA is 18.34% of the mass of EP / N-8OH, and the curing is carried out at 80°C / 6h, and the thermal and mechanical properties after curing are tested.

[0087] Table 3-4 Optimization group test results

[0088]

[0089] Example 4 Characterization of the epoxy resin prepared by the present invention:

[0090] 1 Epoxy value determination

[0091] According to the test standard GB / T 1677-2008, the epoxy value of the product is determined by the hydrochloric acid acetone method. Prepare a mixture of hydrochloric acid and acetone with a volume ratio of 1:40. Add the sample to a conical flask and take 10.00ml of hydrochloric acid acetone solution to dissolve the sample. Let it stand for 30 minutes, add 2 to 3 drops of phenolphthalein indicator, titrate with 0.1mol / L NaOH-ethanol solution standard titrant, and perform a blank test at the same time. Calculate the epoxy value E (mol / 100g) according to formula 2-1.

[0092]

[0093] Where:

[0094] E is the epoxy value, unit: mol / 100g

[0095] c is the actual molar concentration of NaOH-ethanol solution, unit: mol / L

[0096] V1 is the volume of NaOH-ethanol solution consumed by the blank group, unit: ml

[0097] V2 is the volume of NaOH-ethanol solution consumed by the sample, unit: ml

[0098] m is the weight of the sample added to the conical flask (g), unit: g

[0099] 2 Hydroxyl value determination

[0100] According to the test standard GB / T 12008.3-1989, the dianhydride-pyridine method was used to determine the hydroxyl value. 0.28 mol of phthalic anhydride and 300 ml of pyridine were added to a brown bottle to prepare the acetylation reagent. 50 ml of the acetylation reagent was added to a conical flask, and then the sample to be analyzed was placed. A blank group was set up and prepared using 50 ml of the reagent alone, which was treated the same as the solution containing the sample. A reflux condenser was installed in the conical flask, and refluxed at 120 ° C for 2 hours. After the reaction was completed, the system was cooled to room temperature. The condenser and the bottle mouth were washed with 10 ml of pyridine. Titrate with 1 mol / L NaOH-ethanol solution. The hydroxyl value I was calculated according to formula 2-2 (OH) (mgKOH / g).

[0101]

[0102] Where:

[0103] I (OH) Is the hydroxyl value, unit: mgKOH / g

[0104] c is the actual molar concentration of NaOH-ethanol solution, unit: mol / L

[0105] V1 is the volume of blank NaOH-ethanol solution consumed, unit: ml

[0106] V2 is the volume of NaOH-ethanol solution consumed by the sample, unit: ml

[0107] m is the weight of the sample added to the acetylation mixture, unit: g

[0108] In this paper, acetone (AC) and ethyl acetate (EAC) were mixed with different volume ratios to extract the residual ethylene glycol in HEP ​​to prepare high-purity N-8OH, and the hydroxyl value of the product after EG was extracted from HEP by refining the mixed solution was tested. Figure 4As shown. It can be clearly seen that with the increase of ethyl acetate content, the hydroxyl value in the HEP recovery solution decreases, and the EG extraction effect gradually increases. However, when the volume ratio of acetone to ethyl acetate is greater than 14, the hydroxyl value tends to be stable, which means that the EG extraction effect has reached the maximum value. Thereafter, continuing to increase the volume content of EAC has little effect on degradation. Based on the cost and subsequent treatment of AC and EAC, the volume ratio of acetone to ethyl acetate of 1:15 was finally selected as the best compound mixed solution for subsequent recovery (the compound mixed solution is insoluble in octal alcohol, soluble in ethylene glycol, and can extract ethylene glycol from the HEP mixed solution), to achieve complete extraction of residual EG in HEP ​​and prepare high-purity N-8OH.

[0109] 3H NMR spectroscopy ( 1 H NMR)

[0110] The samples were dissolved in deuterated DMSO using a Bruker AMX 600MHz NMR spectrometer and the N-8OH and EP / N-8OH spectra were analyzed at room temperature. 1 H NMR test.

[0111] The NMR hydrogen spectrum of the purified N-8OH is as follows Figure 5 As shown, 1 The structure of N-8OH was verified by HNMR. 1 The specific data of H NMR are as follows: there are double peaks at chemical shifts of 0.96ppm, 0.91ppm and 0.88ppm, which are the methylene proton peaks on the N-8OH heterocyclic structure. They correspond to 2, 3, and 4 in the figure respectively. The chemical shift of 3.21ppm is the methyl proton peak on the carbon connected to the middle hydroxyl group of N-8OH, which is marked 8 in the figure. There is a quartet at this shift; the chemical shift of 3.39ppm corresponds to the mark 10 at N-8OH in the figure, which is the methylene proton peak on the carbon connected to the terminal hydroxyl group. The chemical shifts of 1.06ppm and 0.85ppm correspond to the methyl hydrogen 1 and 5 introduced on the edge of the heterocycle. The hydrogen chemical shifts on the terminal hydroxyl groups of the polyols are 4.89ppm and 5.55ppm, corresponding to 11 and 9 in the figure. The methylene proton peaks adjacent to N are at 2.15ppm and 2.43ppm, and the chemical environments of the two are similar, corresponding to 6 and 7.

[0112] EP / N-8OH 1 H NMR spectrum Figure 6 As shown, with N-8OH 1Compared with the H NMR spectrum, heterocyclic hydrogen also exists at 0.67-0.87ppm, corresponding to 1-4; the chemical shift of 0.62ppm is the methyl hydrogen proton peak on the external carbon of the heterocyclic ring, corresponding to 5, and the methylene proton peak adjacent to N is at 2.15ppm and 2.43ppm, and the two are in similar chemical environments, marked as 6 and 7 in the figure. 3.23ppm is the methyl hydrogen in 8 in the figure. The chemical shifts at 4.38 and 5.54ppm also have hydrogen of terminal hydroxyl groups, corresponding to 14 and 9; there is methylene hydrogen at 3.36ppm, corresponding to 10, which is a proton peak formed by the etherification reaction of the terminal hydroxyl group; there are proton peaks at 3.72, 3.47, and 3.06ppm, corresponding to 12, 11, and 13, which are characteristic proton peaks formed by hydrogen of the synthesized epoxy group. The proton hydrogen at this place is closer to the oxygen atom, and the shielding effect is reduced due to the strong electronegativity of the oxygen heteroatom. Therefore, the signal peak of the proton appears low field. By FT-IR and 1 The successful synthesis of epoxy resin EP / N-8OH was verified by H NMR.

[0113] 4 Infrared spectroscopy (FT-IR)

[0114] 1) DEP infrared spectrum analysis of epoxy resin and alcoholysis solution

[0115] Fourier transform infrared spectrometer (Nicolet-5700) was used to characterize the samples, and the test wavelength range was 4000-500cm -1 The recovery process of alcoholysis solution and the infrared spectra of the products N-8OH and EP / N-8OH were tested at room temperature. The sample was prepared by KBr tablet method.

[0116] FT-IR test spectra of epoxy resin and alcoholysis solution DEP, such as Figure 7 As shown. Figure 7 It can be seen that 1400~1600cm -1 The six-membered ring peak between the two groups shifts after degradation, which is the electronic and steric effect caused by the change of the substituents. -1 、1343cm -1 and 1020cm -1 The strong peak at 756 cm is related to the stretching vibration of the C=O and CO bonds of the ester group. These characteristic peaks are significantly weakened, which proves that the ester bond in EP is degraded after the ester exchange with the EG hydroxyl group. -1 The peak is related to the ortho-substituted stretching vibration of the tetrahydrobenzene ring of EP. From the DEP curve obtained by rotary evaporation to remove the solvent EG, it can be seen that at 3400cm -1 ~3600cm -1 The characteristic peak of hydroxyl group at the site was significantly enhanced, which further illustrates that the EP and IPDA curing part was partially alcoholyzed to generate N-8OH with multi-hydroxyl structure.

[0117] 2) Infrared spectrum of N-8OH refining process

[0118] The FT-IR spectrum of N-8OH refining process is shown in Figure 8 As shown in the figure, 1094cm -1 and 1040cm -1 The characteristic peaks between 1560cm and 1560cm correspond to the primary alcohol and secondary alcohol structures in the polyols. -1 Corresponding to the stretching vibration of CN, it can be seen from the NEP spectrum that after the addition of NaOH, the alkaline hydrolysis reaction is complete. Figure 8 In the DEP, C=O and COC break bonds, 1722 cm -1 and 1193cm -1 At the same time, from the spectra of HEP and N-8OH, we can see that at 3400cm -1 The hydroxyl peak at 1568 cm-1 gradually weakened, indicating that the addition of acetone and ethyl acetate mixed solution to the system can effectively remove residual ethylene glycol. This conclusion was further verified in the determination of hydroxyl value. -1 The peak is the CC skeleton vibration peak of the tetrahydrobenzene ring. It can be seen from the figure that with the addition of ethanol, the sodium salt precipitates from NEP and dissolves in ethanol, and the tetrahydrobenzene ring structure disappears in the obtained product HEP.

[0119] 3) FT-IR test spectra of N-8OH and EP / N-8OH

[0120] The FT-IR test spectra of N-8OH and EP / N-8OH are as follows Fig. 9 As shown in the figure, 3400cm -1 It is the absorption peak of alcoholic hydroxyl. In the FT-IR curve of EP / N-8OH, after calculating the peak area ratio, it is found that the absorption peak of hydroxyl of EP / N-8OH is weakened. This is because the alcoholic hydroxyl of N-8OH has participated in the reaction and has been partially epoxidized. Compared with the FT-IR curve of N-8OH, there is a peak at 910cm in the EP / N-8OH curve. -1 The absorption peak is at 835cm, which is the characteristic absorption peak of the epoxy group (-COC-). -1 The antisymmetric stretching vibration absorption peak of -COC- group is 1077cm -1 The characteristic peak of the stretching vibration absorption of the ether bond (-O-) appeared, indicating that the epoxy group has been successfully connected, and the new glycidyl ether epoxy resin EP / N-8OH has been successfully synthesized. At the same time, more folding segment peaks were introduced, such as at 1552cm -1 The methylene -CH2 deformation vibration absorption peak.

[0121] 5Differential Scanning Calorimetry (DSC)

[0122] The glass transition temperature Tg of EP / N-8OH and EP after curing was tested using a DSC214 differential scanning calorimeter from Mettler Toledo, Switzerland. 5-10 mg of sample was weighed and heated from room temperature to 250°C at a heating rate of 10°C / min in a nitrogen atmosphere.

[0123] 6 Thermogravimetric analysis (TG)

[0124] The weight loss resistance of EP / N-8OH and EP at different temperatures was tested using a STA449F5 thermal analyzer from Netzsch, Germany. 5-10 mg of sample was weighed and placed in a crucible. In a nitrogen atmosphere (50 mL / min), the test temperature was raised from room temperature to 800°C at a rate of 10°C / min.

[0125] 7 Mechanical properties test

[0126] The mechanical properties of the cured specimens were tested using an electronic universal testing machine (ETM-104C) from Shenzhen WanCe Testing Co., Ltd. The test standard was uniformly conducted in accordance with the GB / T 2567-2021 test standard. The tensile specimens were dumbbell-shaped, with a tensile rate of 2 mm / min; the test temperature was 25°C, and the specimen size for the three-point bending performance test and the impact performance test was 80 mm × 10 mm × 4 mm. The test data is the average value of five parallel samples.

[0127] 8 Liquid chromatography-mass spectrometry (LC-MS)

[0128] The molecular weight and distribution of DEP in epoxy resin alcoholysis solution were analyzed using Varian 1200 LC-MS.

[0129] The liquid chromatography-mass spectrometry (LC-MS) of epoxy resin alcoholysis solution DEP was determined experimentally to characterize the molecular weight of DEP components. Fig.10 It can be seen that in the test process, except for an obvious peak at about 0.6min, the peak shapes of other components are basically the same, and no obvious peaks appear. Therefore, the peak position of 0.6min is selected for analysis. Fig.11. The charge-to-mass ratio of 466 is the molecular ion peak of N-8OH in DEP, which proves the existence of N-8OH substance. There are weaker peaks between 500 and 600, indicating that there are still oligomers with incomplete ester bonds during the degradation process of EP. The charge-to-mass ratio of 494 is the fragment ion peak in which the ester bond at one end is not completely broken during the glycolization process of the cured EP. The charge-to-mass ratio of 555 is the substance in which only the ester bond at one end is attacked during the glycolization process of the cured EP, and an ester exchange reaction occurs, and the ester bond is completely broken into a hydroxyl group. The charge-to-mass ratio of 511 is the fragment ion peak in which the ester bond at one end is not completely broken during the glycolization process of the cured EP, and the ester bond at the other end is not degraded. From Fig.10 From the perspective of time, the absolute intensity of the material structure in the spectrum is large, and its molecular weight is distributed within 600. It can be seen that the substances in DEP are all low-molecular-weight degradation products, and the alcoholysis is relatively complete.

[0130] Thermal stability analysis of 9EP / N-8OH

[0131] The TG and DSC analysis of pure EP and EP / N-8OH cured samples showed the following results: Fig.12 The main thermal performance data of EP and EP / N-8OH are listed in Table 3-5. Fig.12 (ab) Combined analysis shows that both EP / N-8OH and EP begin to decompose at around 200°C, and the thermal decomposition curves of the two cured products are slightly different. EP / N-8OH reaches the maximum weight loss rate at around 317.8°C, and EP reaches the maximum weight loss rate at around 333.4°C. This indicates that the main chain of the epoxy group molecule undergoes thermal degradation at this temperature, resulting in rapid weight loss. DSC analysis of the two, such as Fig.12 (c), it can be seen that the glass transition temperature (Tg) of EP is 103°C, and the Tg of EP / N-8OH is 65°C, that is, the thermal stability of the EP / N-8OH cured product synthesized from the recycled polyol is relatively low. This phenomenon may be because in the EP / N-8OH system, the aliphatic long chain of the heterocyclic structure contains abundant terminal hydroxyl groups and terminal epoxy functional groups, which has greater flexibility and gives EP / N-8OH good compatibility, so the thermal stability is reduced compared with the ester epoxy resin cured product before alcoholysis.

[0132] Table 3-5 Thermal analysis test data of EP and EP / N-8OH

[0133]

[0134] 10. Analysis of mechanical properties of EP / N-8OH

[0135] 10.1 Analysis of bending impact performance

[0136] Flexural impact data of EP and EP / N-8OH cured products are as follows: Fig.13 As shown. Fig.13 It can be seen that the impact strength of EP is 11.8KJ / m 2 , the impact strength of EP / N-8OH is 10.3KJ / m 2 . At the same time, the bending strength of EP is 75.7MPa, while the bending strength of EP / N-8OH synthesized by epoxidation is 70.2MPa, which is 7.2% lower than that of EP. Comparative analysis shows that EP has greater bending and impact strength. This may be because the multi-crosslinked structure containing benzene rings and ester bonds in EP provides a higher crosslinking density for epoxy resin. Compared with the fatty chain in the EP / N-8OH molecule, the steric hindrance is large, which provides a more rigid main chain structure for the epoxy resin. Therefore, the entire EP / N-8OH system exhibits lower bending and impact properties than EP.

[0137] 10.2 Tensile performance analysis

[0138] The stress-strain curves of EP and EP / N-8OH cured products are shown in Figure 2. Fig.14 As shown. As can be seen from the figure, the tensile strength of EP is 62.9MPa and the elongation at break is 6.6%. The tensile strength of EP / N-8OH is 56.3MPa, and the elongation at break of EP / N-8OH is 3.0%. Compared with the two, the tensile properties of EP / N-8OH are lower. This may be due to the terminal hydroxyl group and ether bond functional groups contained in the main chain of the molecule after curing of EP / N-8OH synthesized with polyols as monomers, and the large molecular chain mobility, which makes the molecular chain cross-linking density small and the EP / N-8OH curing system has low rigidity. The EP curing molecular structure contains functional groups such as benzene rings and ester bonds. In comparison, the EP / N-8OH structure has a six-membered heterocyclic structure. Therefore, it can be seen from the structure that the chemical steric hindrance of EP is large, and the cross-linking density between the epoxy group and the IPDA curing agent is large. Therefore, the toughness of EP / N-8OH is increased compared to EP epoxy resin, but the relative range of variation is small.

[0139] A comprehensive analysis of the tensile and impact bending properties shows that the mechanical properties of the EP / N-8OH cured product synthesized by N-8OH are lower than those of the EP cured product. The reason may be that EP / N-8OH is an ether epoxy resin with a flexible structure of long fatty chains and contains characteristic heterocyclic six-membered rings and ether bonds and other functional group characteristic structures, while EP is an ester epoxy resin with ester characteristic functional groups connected to benzene rings. The degree of crosslinking between the two after the curing reaction with IPDA is different.

[0140] The present invention uses EG as a solvent, and the hydroxyl group in the EG structure reacts with the ester bond in the TDTMSE solidified material to obtain an ester EP alcoholysis degradation product, and its components are separated and purified. The obtained N-8OH undergoes an etherification ring-closing reaction to synthesize glycidyl ether type EP / N-8OH, thereby realizing the chemical closed-loop recycling of the ester EP degradation product, and the following conclusions are obtained.

[0141] (1) Epoxy resin TDTMSE was cured with IPDA to obtain epoxy resin (EP), and EG was used to perform ester exchange depolymerization reaction on the cured product EP. The obtained alcoholysis solution DEP was subjected to NaOH alkaline cleavage and ethanol was added to extract sodium salt. Finally, the hydroxyl value was used as a standard to extract the residual EG in the degradation solution HEP ​​by exploring the ratio of acetone to ethyl acetate. In this process, when the ratio of acetone to ethyl acetate was 1:15, EG could be completely removed, that is, high-purity N-8OH was obtained. N-8OH was used as a monomer to synthesize a new glycidyl ether type epoxy resin EP / N-8OH. An orthogonal experiment was designed to optimize the etherification process of N-8OH epoxidation to synthesize EP / N-8OH. On the basis of the original NaOH ring-closing reaction at 55°C for 2h, the optimal etherification process conditions for high epoxy value EP / N-8OH were obtained: the molar ratio of polyol to epichlorohydrin was 1:2.2, the catalyst mass was 0.5% of the mass of the polyol, the etherification temperature was 65°C, and the etherification time was 1h. The EP / N-8OH and EP synthesized by this process were cured according to the procedure of 80°C / 6h.

[0142] (2) FT-IR was used to characterize the degradation of EP and the changes in the preparation of N-8OH. 1H NMR was used to analyze the structures of N-8OH and EP / N-8OH; the structure of alcoholysis solution DEP was characterized by liquid chromatography-mass spectrometry; the thermal stability of EP / N-8OH was analyzed by TG and DSC; the mechanical properties of EP / N-8OH were analyzed by tensile, bending and impact tests. The final experimental results showed that both N-8OH and EP / N-8OH achieved the expected structure, and EP / N-8OH had epoxy reaction groups and COC ether bond structures, that is, a new type of glycidyl ether type epoxy resin EP / N-8OH was successfully synthesized in this paper. The test results of the cured samples of EP and EP / N-8OH showed that the thermal decomposition temperature of EP / N-8OH was 317.8℃ and Tg was 65℃ when the curing mass loss rate was the largest. Similarly, the thermal decomposition temperature of EP was 333.4 and Tg was 103℃ when the loss rate was the largest. Compared with pure EP, the thermal stability of EP / N-8OH was reduced, but the relative change was small. The mechanical properties of EP / N-8OH strips such as tensile, bending and impact strength are relatively lower than those of the degraded and cured raw material EP. The tensile strength is reduced from 62.9MPa of EP to 56.3MPa of EP / N-8OH. Similarly, the elongation at break is reduced from 6.6% of EP to 3.0% of EP / N-8OH. At the same time, the impact strength is reduced from 11.8KJ / m 2 Reduced to 10.3KJ / m for EP / N-8OH 2 The bending strength decreases from 75.7 MPa of EP to 70.2 MPa of EP / N-8OH, that is, the synthesized ether EP / N-8OH has greater flexibility.

Claims

1. A polyol N-8OH, Features: The structural formula is shown in Formula I:

2. The method for preparing the polyol N-8OH according to claim 1, Features: It is extracted and separated from the alcoholysis product of thermosetting epoxy resin.

3. The method for preparing polyol N-8OH according to claim 2, Features: The cured epoxy resin is degraded by using ethylene glycol, and the obtained degradation liquid is purified to obtain the polyol N-8OH.

4. The method for preparing the polyol N-8OH according to claim 3, Features: The process route is: The specific steps include: a. Curing of epoxy resin: TDTMSE is used as a monomer and IPDA is used as a curing agent. The two are mixed evenly at room temperature, poured into a mold coated with a silicone release agent, and then vacuum degassed. After the bubbles are removed, the epoxy resin (EP) is cured according to a thermal curing procedure of 80°C / 6h; wherein the mass ratio of the curing agent amount to the monomer amount is 25.5:100; b. Degradation of epoxy resin: EP:ethylene glycol (EG) in a mass ratio of 1:9 was added into a three-necked flask equipped with a condenser, a stirring device, and a heating device, and nitrogen was introduced to exhaust the air in the device, and then the temperature was raised to 180°C for degradation for 3 hours to obtain EP alcoholysis solution (GEP); c. Purification of polyol N-8OH: Remove EG from the alcoholysis solution of EP in step b to obtain a viscous brown mixed solution (DEP); add NaOH for alkaline hydrolysis, the mass of NaOH is 20% of the total mass of DEP, and a 5% NaOH solution is prepared and added to the flask, and the temperature is raised to 60°C for reaction for 2.5 hours. After the reaction is completed, distill off water to obtain a viscous brown mixed solution (NEP); Add anhydrous ethanol to NEP, let stand for 24 hours, filter, take the filtrate and add hydrochloric acid to adjust the pH of the clear liquid to neutral, and obtain a yellow clear filtrate. The filtrate is subjected to rotary evaporation at 80°C to completely remove the ethanol, and a viscous dark red liquid (HEP) is obtained; The residual EG in HEP ​​was extracted by a solvent method to obtain N-8OH, wherein the solvents were ethyl acetate (EAC) and acetone (AC), and the volume ratio of acetone to ethyl acetate was 1:

15.

5. Use of the preparation method of the polyol N-8OH according to any one of claims 2 to 5 in a method for recovering epoxy resin.

6. A glycidyl ether type epoxy resin EP / N-8OH, Features: It is prepared from the polyol N-8OH described in claim 1, and its structural formula is:

7. The glycidyl ether type epoxy resin EP / N-8OH according to claim 6, Features: The invention is prepared by taking polyol N-8OH and epichlorohydrin (ECH) as raw materials and using boron trifluoride etherate (BF3·OEt2) as catalyst, wherein the molar ratio of polyol N-8OH to epichlorohydrin (ECH) is 1:2.1-2.

3.

8. The method for preparing the glycidyl ether type epoxy resin EP / N-8OH according to claim 7, Features: It is prepared from the polyol N-8OH and epichlorohydrin (ECH) as raw materials described in claim 1, and boron trifluoride ethyl ether (BF3·OEt2) as a catalyst, and undergoes ring-opening etherification and alkali-adding ring-closing reaction to obtain a glycidyl ether type epoxy resin EP / N-8OH; the molar ratio of N-8OH to ECH is 1:2.2; and the amount of boron trifluoride ethyl ether (BF3·OEt2) used is 0.5% of the mass of N-8OH. The process route is:

9. The method for preparing the glycidyl ether type epoxy resin EP / N-8OH according to claim 8, Features: It includes the following steps: a. Take N-8OH and ECH in a molar ratio of 1:(2.1-2.3), raise the temperature to 50-80°C, and drop BF with a catalyst mass of 0.3-0.7% of the mass of N-8OH. 3 ·Et 2 O, heat to 80℃ and react for 1-5h to perform etherification ring opening; b. After cooling to 55°C, add 12.5wt% NaOH aqueous solution and react for 2h; c. After the ring closure is completed, dichloroethane (DCE) and distilled water are added to wash until the lower liquid is neutral, and the lower organic phase is retained by separation to obtain a uniform degradation product of the epoxy resin; the ECH and DCE solvents are removed by rotary evaporation to obtain an orange-red viscous liquid, i.e., a new epoxy resin prepolymer EP / N-8OH synthesized from nitrogen-containing polyols; d. Curing: Use EP / N-8OH as monomer and IPDA as curing agent, mix the two thoroughly at room temperature, pour into a mold coated with silicone release agent, and then perform vacuum degassing until there are no bubbles. Complete the curing of EP / N-8OH according to the curing procedure of 80℃ / 6h.

10. The method for preparing the glycidyl ether type epoxy resin EP / N-8OH according to claim 9, Features: The step a is as follows: taking N-8OH and ECH in a molar ratio of 1:2.2, heating to 50°C and adding BF with a catalyst mass of 0.5% of the mass of N-8OH 3 ·Et 2 O, heating to 65°C for 1h to perform etherification ring opening; the curing conditions in step d are: the amount of IPDA is 18.34% of the mass of EP / N-8OH; and curing is performed at 80°C for 6h.