Activity-controllable platinum complex as well as preparation method and application thereof
By introducing amide group and phosphite group coordination compounds into the platinum catalyst, a platinum complex with controllable activity is formed, which solves the problems of activity and stability of the platinum catalyst in the hydrosilylation reaction, and realizes silicone rubber The long-term operability and high catalytic activity ensure the good mechanical properties of silicone rubber.
Patent Information
- Application Number
- CN202410799254.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-20
AI Technical Summary
The existing platinum catalyst has too high activity in the hydrosilylation reaction, resulting in short operation time and poor storage stability. If the activity is too low, the reaction cannot be guaranteed to be complete, and the introduction of inhibitors affects the performance of the silicone rubber.
Introduce amide groups and phosphite groups into the maleic anhydride molecular chain, and use them as coordination compounds to coordinate with platinum together with vinyl siloxane to form a platinum complex with controllable activity to ensure catalytic activity and storage stability. No additional inhibitors are needed.
It achieves stable storage of the platinum catalyst at room temperature and high catalytic activity at high temperatures, ensuring the long-term operability time and good mechanical properties of the silicone rubber and avoiding the use of inhibitors.
Smart Images

Figure BDA0004902868760000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a platinum complex with controllable activity, a preparation method and application thereof. Background Art
[0002] The hydrosilylation reaction has been widely studied in small molecule chemistry. Many transition metal dispersion systems and their complexes can be used to catalyze the hydrosilylation reaction. Among these catalysts, the most effective and widely used is the platinum complex. However, if the activity of the platinum catalyst is too high, there will be problems such as the operating time of the two-component addition-type liquid silicone rubber after mixing is too short, and the single-component addition-type liquid silicone rubber cannot be stored; and if the activity of the catalyst is too low, the addition reaction cannot be guaranteed to be complete. Therefore, improving the catalytic activity and storage stability of the platinum catalyst is of great significance for the synthesis of addition-type silicone rubber.
[0003] In the prior art, the storage stability of platinum catalysts is generally improved by coordinating vinyl siloxane and a compound with an inhibitory effect with platinum to obtain a platinum complex that combines catalysis and inhibition. For example, in the "Preparation Method of a Platinum Catalyst for Liquid Silicone Rubber" disclosed in Chinese patent documents, its publication number is CN107189071A. The invention adopts the method of coordinating divinyltetramethyldisiloxane and maleate compounds with platinum to obtain a special structure platinum catalyst with both catalytic and inhibitory properties; because it can effectively inhibit the occurrence of hydrosilylation reaction at room temperature, it can significantly improve the operability time of addition silicone rubber and the room temperature storage time of single-component addition liquid silicone rubber.
[0004] However, in the prior art, although the coordination of the inhibitory compound with platinum can improve its storage stability at room temperature, it will also have a certain impact on the catalytic activity of the platinum catalyst and the performance of the cured silicone rubber. Summary of the invention
[0005] The present invention aims to overcome the above-mentioned problems existing in the platinum hydrosilylation catalyst in the prior art, and provides a platinum complex with controllable activity, a preparation method thereof and an application thereof. Amide groups and phosphite groups are introduced into the maleic anhydride molecular chain, and the amide groups and the phosphite groups are used as coordination compounds to coordinate with platinum together with vinyl siloxane, so that the storage stability of the platinum catalyst at room temperature can be improved while the catalytic activity for the hydrosilylation reaction can still be maintained at a high level. When the catalyst is used to prepare the catalytic addition type liquid silicone rubber, no inhibitor needs to be added, and the silicone rubber can have better mechanical properties.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a platinum complex with controllable activity, which is formed by the coordination of vinyl siloxane and a modified ligand with chloroplatinic acid; the modified ligand is prepared by the reaction of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite.
[0007] The present invention coordinates vinyl siloxane and modified ligands with chloroplatinic acid to form a platinum complex, so that the platinum complex in the present invention has both catalytic and inhibitory effects on the preparation of addition-type liquid silicone rubber. The modified ligand contains an amide group and a vinyl group obtained by the reaction of maleic anhydride and allylamine, and a phosphite group obtained by the reaction of maleic anhydride and dimethyl hydroxymethyl phosphite; the introduction of each functional group in the modified ligand allows the platinum complex in the present invention to be stably stored at room temperature in silicone rubber, and has a long operable time when used to prepare addition-type liquid silicone rubber; at the same time, the introduction of each functional group can also ensure that the platinum complex has high catalytic activity and can quickly catalyze the hydrosilylation reaction at high temperature. When the platinum complex in the present invention is used in the preparation of addition-type liquid silicone rubber, there is no need to add an inhibitor, and it can ensure that the silicone rubber obtained after curing has good mechanical properties.
[0008] Preferably, the molar ratio of chloroplatinic acid to vinyl siloxane is 1:3-50, and the molar ratio of the modified ligand to vinyl siloxane is 1:5-50.
[0009] Preferably, the vinyl siloxane is one or more of tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and vinyl-terminated silicone oil.
[0010] Preferably, the molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethylphosphite is 1:1-1.2:1-1.2.
[0011] In a second aspect, the present invention provides a method for preparing the above-mentioned platinum complex with controllable activity, comprising the following steps: (1) reacting maleic anhydride with allylamine, and then reacting the product with dimethyl hydroxymethylphosphite to obtain a modified ligand; (2) dissolving sodium bicarbonate in an alcohol solvent, and then adding chloroplatinic acid and vinyl siloxane to the solution for heating reaction; (3) mixing the product obtained in step (2) with the modified ligand, and heating the mixture to obtain the platinum complex with controllable activity.
[0012] Preferably, the reaction conditions of maleic anhydride and allylamine in step (1) are: adding maleic anhydride to a solvent, then heating the solution to 35-50° C., adding allylamine dropwise to the solution, reacting for 1-2 hours, and removing the solvent.
[0013] Preferably, the reaction conditions of the product obtained by the reaction of maleic anhydride and allylamine with dimethyl hydroxymethyl phosphite in step (1) are as follows: the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and sodium methoxide catalyst is added, and the reaction is carried out at 120-160° C. for 3-8 hours, and the modified ligand is obtained after removing the solvent.
[0014] Preferably, the alcohol solvent described in step (2) is one or more of methanol, ethanol, and isopropanol; and the mass ratio of the added sodium bicarbonate to chloroplatinic acid is 2 to 5:1.
[0015] Preferably, the reaction temperature of step (2) is 40-80°C, and the reaction time is 1-4h; the reaction temperature of step (3) is 50-100°C, and the reaction time is 0.5-2h.
[0016] In a third aspect, the present invention provides a use of the above-mentioned platinum complex with controllable activity in the preparation of silicone rubber.
[0017] Therefore, the present invention has the following beneficial effects: vinyl siloxane and a modified ligand are coordinated with chloroplatinic acid to form a platinum complex, and functional groups such as amide, phosphite, and vinyl are introduced into the modified ligand, so that the platinum complex in the present invention has both catalytic and inhibitory effects on the preparation of addition-type liquid silicone rubber, can be stably stored in silicone rubber at room temperature, and has a long operable time when used for preparing addition-type liquid silicone rubber; at the same time, the introduction of each functional group can also ensure that the platinum complex has high catalytic activity, and can quickly catalyze the hydrosilylation reaction at high temperature; when the platinum complex in the present invention is used for the preparation of addition-type liquid silicone rubber, there is no need to add an inhibitor, and it can be ensured that the silicone rubber obtained after curing has good mechanical properties. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with specific implementation methods.
[0019] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are conventional methods in the art.
[0020] Overall embodiment: A platinum complex with controllable activity is formed by the coordination of vinyl siloxane and a modified ligand with chloroplatinic acid; the modified ligand is prepared by the reaction of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite.
[0021] The above-mentioned vinyl siloxane is one or more of tetramethyl divinyl disiloxane, tetramethyl tetravinyl cyclotetrasiloxane, and vinyl-terminated silicone oil; preferably tetramethyl divinyl disiloxane. The viscosity of the vinyl-terminated silicone oil is 5 to 50 mm 2 / s.
[0022] When the above-mentioned modified ligand is prepared, the molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite is 1:1-1.2:1-1.2; in certain specific embodiments of the present invention, when the modified ligand is prepared, the molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite is 1:1:1, 1:1:1.1, 1:1:1.2, 1:1.1:1, 1:1.2:1 or 1:1.1:1.1.
[0023] In the present invention, the molar ratio of chloroplatinic acid to vinyl siloxane is 1:3-50, and the molar ratio of the modified ligand to vinyl siloxane is 1:5-50; preferably, the molar ratio of chloroplatinic acid to vinyl siloxane is 1:5-30, and the molar ratio of the modified ligand to vinyl siloxane is 1:5-30; more preferably, the molar ratio of chloroplatinic acid to vinyl siloxane is 1:10-20, and the molar ratio of the modified ligand to vinyl siloxane is 1:5-10; in certain specific embodiments of the present invention, the molar ratio of chloroplatinic acid to vinyl siloxane is 1:5, 1:10, 1:15 or 1:20, and the molar ratio of the modified ligand to vinyl siloxane is 1:5, 1:10 or 1:15.
[0024] The method for preparing the above-mentioned platinum complex with controllable activity comprises the following steps: (1) reacting maleic anhydride with allylamine, and then reacting the product with dimethyl hydroxymethylphosphite to obtain a modified ligand; (2) dissolving sodium bicarbonate in an alcohol solvent, and then adding chloroplatinic acid and vinyl siloxane to the solution for heating reaction; (3) mixing the product obtained in step (2) with the modified ligand, and heating the mixture to obtain the platinum complex with controllable activity.
[0025] The reaction conditions of maleic anhydride and allylamine in step (1) are: adding maleic anhydride to a solvent, then heating the solution to 35-50°C, dropping allylamine into the solution, reacting for 1-2 hours, and removing the solvent. In the present invention, the solvent is water or ethanol; the method of removing the solvent is vacuum distillation, and the present invention has no special restrictions on the method and equipment of the vacuum distillation, and the method and equipment familiar to those skilled in the art can be used; the present invention has no special restrictions on the heating method, and water bath heating or oil bath heating is preferred.
[0026] The reaction conditions of the product obtained by the reaction of maleic anhydride and allylamine with dimethyl hydroxymethyl phosphite in step (1) are as follows: the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and sodium methoxide catalyst is added, and the reaction is carried out at 120-160° C. for 3-8 hours, and the modified ligand is obtained after the solvent is removed. In the present invention, the amount of sodium methoxide catalyst added is 10-100 ppm, preferably 30-50 ppm; in the present invention, the method for removing the solvent is vacuum distillation, and the present invention has no special restrictions on the method and equipment of the vacuum distillation, and the method and equipment well known to those skilled in the art can be used.
[0027] The alcohol solvent described in step (2) is one or more of methanol, ethanol, and isopropanol; preferably ethanol or isopropanol; in the present invention, the mass ratio of the added sodium bicarbonate to chloroplatinic acid is 2 to 5:1.
[0028] In the present invention, the reaction temperature of step (2) is 40-80°C, preferably 45-55°C; the reaction time of step (2) is 1-4h, preferably 1-2h; in the present invention, the reaction temperature of step (3) is 50-100°C, preferably 60-80°C; the reaction time of step (3) is 0.5-2h, preferably 1-1.5h; the present invention has no special restrictions on the heating method, preferably water bath heating or oil bath heating.
[0029] In the present invention, step (3) further comprises the steps of filtering to remove solid matter in the product and removing low-boiling substances by vacuum distillation after the heating reaction; the present invention has no special limitation on the method and equipment of the vacuum distillation, and the method and equipment familiar to those skilled in the art can be used.
[0030] In the present invention, the reactions of step (2) and step (3) are carried out under the protection of an inert gas, and the inert gas is preferably nitrogen.
[0031] Embodiment 1: A method for preparing a platinum complex with controllable activity, comprising the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of the added maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite is 1:1:1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for a reaction of 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex with controllable activity.
[0032] Embodiment 2: A method for preparing a platinum complex with controllable activity, comprising the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite added is 1:1:1.1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:10, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex with controllable activity.
[0033] Embodiment 3: A method for preparing a platinum complex with controllable activity, comprising the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of the added maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite is 1:1:1.2; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:15, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex with controllable activity.
[0034] Embodiment 4: A method for preparing a platinum complex with controllable activity, comprising the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite added is 1:1.1:1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:20, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex with controllable activity.
[0035] Embodiment 5: A method for preparing a platinum complex with controllable activity, comprising the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite added is 1:1.2:1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for a reaction of 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:10, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex with controllable activity.
[0036] Embodiment 6: A method for preparing a platinum complex with controllable activity, comprising the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of the added maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite is 1:1.1:1.1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for a reaction of 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:15, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex with controllable activity.
[0037] Comparative Example 1 (without adding modified ligand): A method for preparing a platinum complex comprises the following steps: Sodium bicarbonate is dissolved in ethanol, nitrogen is passed through the solution to deoxygenate it, and then chloroplatinic acid and tetramethyldivinyldisiloxane are added to the solution. After heating at 50° C. for 1.5 hours, the solid matter in the product is filtered out and low-boiling substances are removed by reduced pressure distillation to obtain the platinum complex; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1.
[0038] Comparative Example 2 (no phosphite group is introduced into the modified ligand): A method for preparing a platinum complex comprises the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., allylamine is added dropwise to the solution, and after reacting for 2 hours, the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of the added maleic anhydride to the allylamine is 1:1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for a reaction of 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex.
[0039] Comparative Example 3 (Amide groups are not introduced into the modified ligand): A method for preparing a platinum complex comprises the following steps: (1) adding maleic anhydride and dimethyl hydroxymethyl phosphite to xylene, and adding 5 ppm sodium methoxide catalyst, reacting at 130° C. for 5 hours, and removing the solvent under reduced pressure to obtain a modified ligand; the molar ratio of the added maleic anhydride to the dimethyl hydroxymethyl phosphite is 1:1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for a reaction of 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex.
[0040] Comparative Example 4 (changing the type of primary amine reacting with maleic anhydride): A method for preparing a platinum complex comprises the following steps: (1) maleic anhydride is added to water to dissolve, and then the solution is heated to 40° C., n-propylamine is added dropwise to the solution, and the solvent is removed under reduced pressure after reacting for 2 hours; the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and 5 ppm sodium methoxide catalyst is added, and the reaction is carried out at 130° C. for 5 hours, and the solvent is removed under reduced pressure to obtain a modified ligand; the molar ratio of the added maleic anhydride, n-propylamine and dimethyl hydroxymethyl phosphite is 1:1:1; (2) dissolving sodium bicarbonate in ethanol, passing nitrogen gas through the solution to deoxygenate it, adding chloroplatinic acid and tetramethyldivinyldisiloxane to the solution, and heating the solution at 50° C. for a reaction of 1.5 h; the molar ratio of chloroplatinic acid to tetramethyldivinyldisiloxane is 1:5, and the mass ratio of sodium bicarbonate to chloroplatinic acid is 3:1; (3) mixing the product obtained in step (2) with the modified ligand obtained in step (1), wherein the molar ratio of the modified ligand to tetramethyldivinyldisiloxane is 1:5, heating the mixture at 70° C. for 1 h, filtering to remove solid matter from the product, and removing low-boiling substances by distillation under reduced pressure to obtain the platinum complex.
[0041] Vinyl silicone oil with a double bond content of 2% and hydrogen-containing silicone oil with a hydrogen content of 1% were mixed, and the platinum complexes prepared in the above embodiments and comparative examples were added respectively, the mass of platinum in the platinum complex was 5ppm of the mass of the vinyl silicone oil, and the mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil was 100:5. After being mixed evenly, the mixture was reacted at 120° C. for 10 minutes to obtain silicone rubber. In comparative example 1, in addition to the platinum complex, an inhibitor, ethynyl cyclohexanol, was also added, and the mass ratio of the inhibitor to the vinyl silicone oil was 0.3:100. No inhibitor was added to the other embodiments and comparative examples.
[0042] The vulcanization performance and mechanical properties of silicone rubber were tested, and the results are shown in Table 1. The test method for the vulcanization performance is as follows: the prepared silicone rubber is placed in a rotorless vulcanizer, and the vulcanization test is performed at 120°C to measure the time T50 and T90 required for the rubber to reach 50% and 90% of the maximum torque to evaluate the activity of the platinum complex; the shorter the time, the faster the vulcanization speed and the higher the activity of the platinum complex. The test method for the mechanical properties of silicone rubber refers to GB / T528-2009.
[0043] Table 1: Silicone rubber performance test results.
[0044] Vinyl silicone oil with a double bond content of 2% and hydrogen-containing silicone oil with a hydrogen content of 1% were mixed, and the platinum complexes prepared in the above embodiments and comparative examples were added respectively, the mass of platinum in the platinum complex was 5 ppm of the mass of the vinyl silicone oil, and the mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil was 100:5 (an inhibitor was also added in Comparative Example 1). After mixing evenly, the sample was sealed and placed in an environment of 25° C. The time taken for the viscosity to increase to twice the initial viscosity was tested to reflect the room temperature catalytic activity of the platinum complex. The results are shown in Table 2.
[0045] Table 2: Room temperature catalytic activity test results. serial number Initial viscosity (mPa·s) Final viscosity (mPa·s) Time taken (days) Example 1 28100 56700 91 Example 2 27300 54800 94 Example 3 26700 53600 96 Example 4 25900 52300 105 Example 5 27800 55900 93 Example 6 27700 55500 96 Comparative Example 1 27800 56000 4 Comparative Example 2 28200 56600 33 Comparative Example 3 27900 55900 126 Comparative Example 4 28000 56300 117
[0046] It can be seen from Table 1 and Table 2 that the platinum complexes prepared by the method of the present invention in Examples 1 to 6 have low catalytic activity at room temperature, can be stably stored in silicone rubber, and do not require the addition of inhibitors when catalyzing the preparation of silicone rubber, and have a long operable time; and can quickly catalyze the hydrosilylation reaction at high temperatures, have high catalytic activity, and the silicone rubber prepared by catalysis has good mechanical properties.
[0047] In Comparative Example 1, no modified ligand is added to coordinate with chloroplatinic acid, and the obtained platinum complex has no inhibitory properties. It is difficult to store stably in silicone rubber at room temperature. An external inhibitor is required when preparing silicone rubber, and the operation time is short. In Comparative Example 2, no phosphate group is introduced into the modified ligand, and the storage stability of the platinum complex is significantly reduced compared with that in the example. In Comparative Example 3, no amide group and vinyl group in allylamine are introduced into the modified ligand, and the high-temperature catalytic activity of the catalyst is significantly reduced compared with that in the example, resulting in a decrease in the mechanical properties of the silicone rubber finally obtained. In Comparative Example 4, n-propylamine is used instead of allylamine for reaction, and the introduction of vinyl group is lacking, and the high-temperature catalytic activity of the catalyst and the mechanical properties of the silicone rubber are also reduced.
Claims
1. A platinum complex with controllable activity, characterized in that: The invention is formed by the coordination of vinyl siloxane and a modified ligand with chloroplatinic acid; the modified ligand is prepared by the reaction of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite.
2. The platinum complex with controllable activity according to claim 1, characterized in that: The molar ratio of chloroplatinic acid to vinyl siloxane is 1:3-50, and the molar ratio of the modified ligand to vinyl siloxane is 1:5-50.
3. The controllable activity platinum complex according to claim 1 or 2, characterized in that: The vinyl siloxane is one or more of tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and vinyl-terminated silicone oil.
4. The platinum complex with controllable activity according to claim 1, characterized in that: The molar ratio of maleic anhydride, allylamine and dimethyl hydroxymethyl phosphite is 1:1~1.2: 1~1.
2.
5. A method for preparing a platinum complex with controllable activity as claimed in any one of claims 1 to 4, characterized in that: The steps include: (1) reacting maleic anhydride with allylamine, and then reacting the product with dimethyl hydroxymethyl phosphite to obtain a modified ligand; (2) dissolving sodium bicarbonate in an alcohol solvent, then adding chloroplatinic acid and vinyl siloxane to the solution and heating the solution for reaction; (3) The product obtained in step (2) is mixed with the modified ligand, and heated to react to obtain the platinum complex with controllable activity.
6. The preparation method according to claim 5, characterized in that: The reaction conditions of maleic anhydride and allylamine in step (1) are as follows: maleic anhydride is added to a solvent, the solution is then heated to 35-50° C., allylamine is added dropwise to the solution, and the solvent is removed after reacting for 1-2 hours.
7. The preparation method according to claim 5 or 6, characterized in that: The reaction conditions of the product obtained by the reaction of maleic anhydride and allylamine with dimethyl hydroxymethyl phosphite in step (1) are as follows: the obtained product and dimethyl hydroxymethyl phosphite are added to xylene, and sodium methoxide catalyst is added, and the reaction is carried out at 120-160° C. for 3-8 hours, and the modified ligand is obtained after removing the solvent.
8. The preparation method according to claim 5, characterized in that: The alcohol solvent described in step (2) is one or more of methanol, ethanol, and isopropanol; the mass ratio of the added sodium bicarbonate to chloroplatinic acid is 2-5:
1.
9. The preparation method according to claim 5 or 8, characterized in that: The reaction temperature of step (2) is 40-80°C; the reaction temperature of step (3) is 50-100°C.
10. Use of the platinum complex with controllable activity as claimed in any one of claims 1 to 4 in the preparation of silicone rubber.
Citation Information
Patent Citations
PVC (polyvinyl chloride) / styrene polymer alloy and preparation method thereof
CN102731936A
Preparation method of silane coupling agent with imide cycle structural unit
CN103665020A
Preparation method of platinum catalyst for liquid silicone rubber
CN107189071A
Preparation method and application of high-stability platinum catalyst for hydrosilylation
CN112961192A
Composition for producing polyacrylic ester and production of polycrylic ester