Reactive block plasticizer and modified PLA low-temperature shrink film thereof

By introducing a reactive block plasticizer into PLA for grafting reaction, an ABA-type structure is formed, which solves the problem of poor aging resistance of PLA low-temperature shrink film and achieves high light transmittance and long-term performance stability of the modified PLA low-temperature shrink film. sex.

CN118725183APending Publication Date: 2024-10-01JIANGSU JINGHONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410943777.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

PLA low-temperature shrink film has poor aging resistance and is prone to rapid performance degradation due to migration and volatilization of small molecule plasticizers.

Method used

Reactive block plasticizer is used to introduce epoxy groups into PLA for grafting reaction to form an ABA type hard segment-soft segment-hard segment block structure, which enhances the chemical anchoring effect with PLA and is prepared by combining spray drying. Powder for modified PLA low temperature shrink film.

Benefits of technology

It effectively overcomes the migration problem of small molecule plasticizers, maintains the light transmittance and soft feel of the modified PLA low-temperature shrink film, and improves long-term performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945002530000041
    Figure BDA0004945002530000041
  • Figure BDA0004945002530000042
    Figure BDA0004945002530000042
  • Figure BDA0004945002530000101
    Figure BDA0004945002530000101
Patent Text Reader

Abstract

The invention relates to the technical field of shrink films, in particular to a reactive block plasticizer and a modified PLA low-temperature shrink film thereof. According to a small-molecule plasticizer modified PLA low-temperature shrink film, a small-molecule plasticizer is easy to migrate to the surface of a material, and the ageing resistance of the shrink film is relatively poor. Aiming at the problems, the invention provides the reactive block plasticizer, the molecular structure of the reactive block plasticizer contains an epoxy group, and the reactive block plasticizer can be subjected to grafting reaction with hydroxyl or carboxyl on the molecular structure of PLA during high-temperature blending, so that the molecular chain of the reactive block plasticizer is introduced into a PLA matrix resin structure, and the problem that a small-molecular plasticizer is easy to migrate to the surface of a material is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shrinkage films, and in particular to a reactive block plasticizer and a modified PLA low-temperature shrinkage film thereof. Background Art

[0002] Polylactic acid (PLA), as a bio-based degradable polymer, has attracted widespread attention due to its renewable source and good biocompatibility.

[0003] PLA low temperature shrink film has high transparency, good mechanical properties, adjustable heat shrinkage rate, etc. It can be used in food packaging, electronic product packaging, heat shrink labels, etc.

[0004] However, PLA has problems such as high brittleness, poor heat resistance, and easy shrinkage and deformation, which limit its application in the field of low-temperature shrink films. In order to solve the above problems, the conventional method is to add small molecule plasticizers to PLA to improve its flexibility, but these plasticizers are easy to migrate and volatilize, resulting in rapid deterioration of the performance of PLA materials over time and poor aging resistance. Summary of the invention

[0005] The problem in the prior art is that the PLA low-temperature shrink film modified by a small molecule plasticizer has poor aging resistance. In view of the above problem, the present invention provides a reactive block plasticizer, wherein the reaction raw materials, in parts by weight, include the following components:

[0006] Emulsifier 2.4-5 parts;

[0007] 120-150 parts of hard segment monomer;

[0008] Internal plasticizing monomer 150-180 parts;

[0009] 6-9 copies of functional monomer;

[0010] 3-9 parts of cross-linking monomer;

[0011] Initiator 1.5-2.1 parts;

[0012] 3-6 parts of neutralizer;

[0013] Reducing agent 0.5-0.8 parts;

[0014] 250-300 parts of deionized water.

[0015] Preferably, the emulsifier includes one or more of Adeka REASOAPSR-10, REACTSURF S8115, and GEROPON DES30.

[0016] Preferably, the hard segment monomer includes one or more of methyl methacrylate, styrene, isobornyl methacrylate, and glycidyl methacrylate.

[0017] Preferably, the internal plasticizing monomer includes one or more of di-n-butyl itaconate, dioctyl maleate, dibutyl fumarate, butyl acrylate, and isooctyl acrylate.

[0018] Preferably, the functional monomer includes one or more of methacrylic acid, acrylic acid, and β-acryloxypropionic acid.

[0019] Preferably, the cross-linking monomer includes one or more of tripropylene glycol diacrylate (TPGDA), trimethylolpropane triacrylate (TMPTA), 1,6-hexanediol diacrylate (HDDA), and diethylene glycol dimethacrylate (DEGDMA).

[0020] Preferably, the initiator comprises potassium persulfate or ammonium persulfate.

[0021] Preferably, the neutralizing agent comprises aqueous ammonia, triethylamine or dimethylethanolamine.

[0022] Preferably, the reducing agent is a sodium salt of an organic sulfinic acid derivative.

[0023] Preferably, the sodium salt of the organic sulfinic acid derivative includes one or more of disodium hydroxyacetic acid sulfinate, sodium benzene sulfinate, and sodium methane sulfinate.

[0024] Preferably, the preparation method of the reactive block plasticizer comprises the following steps:

[0025] S1, dissolving the formulated amount of initiator in 1 / 20 of the formulated amount of deionized water to obtain an initiator solution;

[0026] Adding a formula amount of reducing agent to 1 / 20 of the formula amount of deionized water to obtain a reducing agent solution;

[0027] S2. Preparation of monomer pre-emulsion A

[0028] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of hard segment monomer, 1 / 2 of the formula amount of cross-linking monomer, 1 / 2 of the formula amount of functional monomer, 1 / 3 of the formula amount of initiator solution, and 1 / 4 of the formula amount of neutralizer are sequentially added thereto, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion A;

[0029] S3, preparation of monomer pre-emulsion B

[0030] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of internal plasticizer monomer, the remaining formula amount of cross-linking monomer, the remaining formula amount of functional monomer, 1 / 3 weight part of initiator solution, and 1 / 4 weight part of neutralizer are added thereto in sequence, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion solution B;

[0031] S4. Preparation of reactive internal plasticizing monomer resin emulsion

[0032] Heat the remaining amount of deionized water to 80°C, add the remaining amount of emulsifier, add 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution, stir and react at constant temperature for 20 minutes, then add 50% by weight of the remaining monomer pre-emulsion A dropwise while stirring within 0.5h-1.5h. After the reaction is completed, immediately add all of the monomer pre-emulsion B dropwise while stirring within 1h-1.5h. After the reaction is completed, immediately add the remaining weight of the monomer pre-emulsion B dropwise while stirring within 0.5h-1.5h. After the addition of monomer pre-emulsion A is completed, the mixture is stirred at a constant temperature of 85°C for 1 hour. After the reaction is completed, the temperature of the reaction system is lowered to 60-65°C. After that, the whole reducing agent solution is continuously added dropwise while stirring, and the addition is completed within 1 hour. After that, the mixture is stirred at a constant temperature for 0.5-1 hour. After that, the temperature of the reaction system is lowered to room temperature, and the remaining amount of neutralizer is added. After stirring for 0.5 hour, the reaction solution is filtered with a 240-mesh filter to obtain a reactive block plasticizer emulsion with an average particle size range of 50-150 nm.

[0033] S5. Preparation of reactive internal plasticizing monomer resin powder

[0034] The reactive block plasticizer emulsion obtained in step S4 is subjected to high-speed centrifugation and spray drying to be made into powder, thereby obtaining a reactive block plasticizer having an ABA type hard segment-soft segment-hard segment block structure, wherein the A segment is an epoxy acrylate copolymer segment, and the B segment is an internal plasticizer monomer copolymer segment.

[0035] Preferably, the centrifugal speed is 18000-20000 rpm, the inlet temperature of the spray drying is 140°C-160°C, and the outlet temperature is 80-90°C.

[0036] A modified PLA low-temperature shrink film, comprising the following components in parts by weight:

[0037] PLA 600-750 parts;

[0038] 10-60 parts of reactive block plasticizer;

[0039] 1-3 parts of lubricant;

[0040] Anti-aging agent 0.5-1 part.

[0041] Preferably, the molecular weight of the PLA is 150,000-160,000 Mw.

[0042] Preferably, the lubricant is a mixture of erucamide and zinc stearate in a mass ratio of 1-5:1, and the antioxidant is a mixture of antioxidant 168 and antioxidant 1010 in a mass ratio of 1-2:1.

[0043] Preferably, the preparation method of the modified PLA low-temperature shrink film comprises the following steps:

[0044] Step 1, according to the formula amount, PLA, reactive block plasticizer, lubricant, and anti-aging agent are uniformly blended to obtain a mixed material, and then the mixed material is added to a twin-screw extruder, heated and melt-blended, and then extruded and cast through a die head of the twin-screw extruder to obtain a cast sheet;

[0045] Step 2, biaxially stretching the cast sheet obtained in step (1), first longitudinally stretching and then transversely stretching, and then heat-setting to obtain a modified PLA low-temperature shrink film.

[0046] Preferably, in step (1), the blending stirring speed is 600-800 rpm, the blending time is 20-30 min, the melt blending temperature is 160-190° C., the temperature of the twin-screw extruder die is 200-210° C., the temperature of the casting roll is 35-55° C., the temperature of the biaxial stretching is controlled to be 50-70° C., the stretching speed is controlled to be 50-100 mm / s, the stretching ratio is 3-6, and the heat setting temperature is 100-120° C.

[0047] The present invention has the following beneficial effects:

[0048] (1) The reactive block plasticizer obtained in the present invention contains epoxy groups in its molecular structure, which can undergo a grafting reaction with the hydroxyl or carboxyl groups on the PLA molecular structure during high-temperature blending, thereby introducing its molecular chain into the PLA matrix resin structure, effectively overcoming the problem that small molecule plasticizers are prone to migrate to the material surface;

[0049] (2) The refractive index of the reactive block plasticizer obtained in the present invention is similar to that of PLA. This property ensures that the obtained modified PLA low-temperature shrink film still has excellent light transmittance, effectively reduces the occurrence of atomization, and has good optical clarity;

[0050] (3) The reactive block plasticizer obtained in the present invention is tightly combined with the PLA matrix by chemical grafting. This chemical anchoring effect not only gives the obtained modified PLA low-temperature shrink film a softer feel, but also ensures the long-term performance stability of the film. DETAILED DESCRIPTION

[0051] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0052] The PLA in the following examples of the present invention was purchased from Zhejiang Hisun Biomaterials Co., Ltd., with the brand name REVODE110.

[0053] Example 1

[0054] A modified PLA low-temperature shrink film, the ingredients of which are as follows, measured in parts by weight:

[0055]

[0056] The raw materials of the reactive block plasticizer are composed of the following in parts by weight:

[0057]

[0058] The emulsifier is prepared by mixing emulsifier REACTSURF S8115 and emulsifier DES-30 in a weight ratio of 1:2.

[0059] The hard segment monomer is a mixture of methyl methacrylate and glycidyl methacrylate in a weight ratio of 3:2.

[0060] The internal plasticizing monomer is a mixture of isooctyl acrylate and dioctyl maleate in a weight ratio of 1:1.

[0061] The functional monomer is methacrylic acid.

[0062] The cross-linking monomer is TMPTA.

[0063] The initiator is ammonium persulfate.

[0064] The neutralizing agent is dimethylethanolamine.

[0065] The reducing agent is disodium glycolate sulfinate.

[0066] The lubricant is prepared by mixing erucamide and zinc stearate in a mass ratio of 1:1, and the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 2:1.

[0067] The reactive block plasticizer is prepared by the following method:

[0068] S1, dissolving the formulated amount of initiator in 1 / 20 of the formulated amount of deionized water to obtain an initiator solution;

[0069] Adding a formula amount of reducing agent to 1 / 20 of the formula amount of deionized water to obtain a reducing agent solution;

[0070] S2. Preparation of monomer pre-emulsion A

[0071] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of hard segment monomer, 1 / 2 of the formula amount of cross-linking monomer, 1 / 2 of the formula amount of functional monomer, 1 / 3 of the formula amount of initiator solution, and 1 / 4 of the formula amount of neutralizer are sequentially added thereto, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion A;

[0072] S3, preparation of monomer pre-emulsion B

[0073] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of internal plasticizer monomer, the remaining formula amount of cross-linking monomer, the remaining formula amount of functional monomer, 1 / 3 weight part of initiator solution, and 1 / 4 weight part of neutralizer are added thereto in sequence, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion solution B;

[0074] S4. Preparation of reactive internal plasticizing monomer resin emulsion

[0075] Heat the remaining amount of deionized water to 80°C, add the remaining amount of emulsifier, add 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution, stir and react at constant temperature for 20 minutes, then add 50% by weight of the remaining monomer pre-emulsion A dropwise within 0.5h while stirring. After the reaction is completed, immediately add all of the monomer pre-emulsion B dropwise within 1h while stirring. After the reaction is completed, immediately add the remaining weight of the monomer pre-emulsion B dropwise within 0.5h while stirring. After the addition of liquid A is completed, the mixture is stirred at a constant temperature of 85°C for 1 hour. After the reaction is completed, the temperature of the reaction system is lowered to 60°C. Then, all the reducing agent solution is continuously added dropwise while stirring, and the addition is completed within 1 hour. Then, the mixture is stirred at a constant temperature for 0.5 hour. Then, the temperature of the reaction system is lowered to room temperature, and the remaining amount of the neutralizing agent is added. After stirring for 0.5 hour, the reaction solution is filtered with a 240-mesh filter to obtain a reactive block plasticizer emulsion with a particle size range of 50-150 nm.

[0076] S5. Preparation of reactive internal plasticizing monomer resin powder

[0077] The reactive block plasticizer emulsion obtained in step S4 is subjected to high-speed centrifugation and spray drying to obtain a powder, i.e., a reactive block plasticizer having an ABA type hard segment-soft segment-hard segment block structure, wherein the A segment is an epoxy acrylate copolymer segment, and the B segment is an internal plasticizing monomer copolymer segment. The centrifugal speed is 18000 rpm, the spray drying inlet temperature is 140° C., and the outlet temperature is 80° C.

[0078] The modified PLA low-temperature shrink film is prepared by the following method:

[0079] Step 1, according to the formula amount, PLA, reactive block plasticizer, lubricant, and anti-aging agent are uniformly blended to obtain a mixed material, and then the mixed material is added to a twin-screw extruder, heated and melt-blended, and then extruded and cast through a die head of the twin-screw extruder to obtain a cast sheet;

[0080] Step 2, biaxially stretching the cast sheet obtained in step (1), first longitudinally stretching and then transversely stretching, and then heat-setting to obtain a modified PLA low-temperature shrink film.

[0081] In step (1), the blending stirring speed is 600 rpm, the blending time is 20 min, the melt blending temperature is 160° C., the temperature of the twin-screw extruder die head is 200° C., and the temperature of the casting roll is 35° C.

[0082] In step (2), the temperature of biaxial stretching is controlled at 50°C, the stretching speed is controlled at 50 mm / s, the stretching ratio is 3, and the heat setting temperature is 100°C.

[0083] Example 2

[0084] A modified PLA low-temperature shrink film, which has the following components in parts by weight:

[0085] PLA 650 copies;

[0086] 30 parts of reactive block plasticizer;

[0087] 1.5 parts of lubricant;

[0088] 0.5 parts of anti-aging agent.

[0089] The raw materials of the reactive block plasticizer are composed of the following in parts by weight:

[0090] 4 parts of emulsifier;

[0091] 150 parts of hard segment monomer;

[0092] Internal plasticizing monomer 180 parts;

[0093] 6 parts of functional monomer;

[0094] 9 parts of cross-linking monomer;

[0095] 2.1 parts of initiator;

[0096] 5 parts of neutralizer;

[0097] 0.8 part of reducing agent;

[0098] 300 parts of deionized water.

[0099] The lubricant is prepared by mixing erucamide and zinc stearate in a mass ratio of 1:1, and the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 2:1.

[0100] The emulsifier is prepared by mixing emulsifier REACTSURF S8115 and emulsifier DES-30 in a weight ratio of 1:2.

[0101] The hard segment monomer is a mixture of styrene and glycidyl methacrylate in a weight ratio of 2:1.

[0102] The internal plasticizing monomer is a mixture of butyl acrylate and dioctyl maleate in a weight ratio of 1:1.

[0103] The functional monomer is acrylic acid.

[0104] The cross-linking monomer is TPGDA.

[0105] The initiator is ammonium persulfate.

[0106] The neutralizing agent is dimethylethanolamine.

[0107] The reducing agent is disodium glycolate sulfinate.

[0108] The reactive block plasticizer is prepared by the following method:

[0109] S1, dissolving the formulated amount of initiator in 1 / 20 of the formulated amount of deionized water to obtain an initiator solution;

[0110] Adding a formula amount of reducing agent to 1 / 20 of the formula amount of deionized water to obtain a reducing agent solution;

[0111] S2. Preparation of monomer pre-emulsion A

[0112] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of hard segment monomer, 1 / 2 of the formula amount of cross-linking monomer, 1 / 2 of the formula amount of functional monomer, 1 / 3 of the formula amount of initiator solution, and 1 / 4 of the formula amount of neutralizer are sequentially added thereto, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion A;

[0113] S3, preparation of monomer pre-emulsion B

[0114] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of internal plasticizer monomer, the remaining formula amount of cross-linking monomer, the remaining formula amount of functional monomer, 1 / 3 weight part of initiator solution, and 1 / 4 weight part of neutralizer are added thereto in sequence, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion solution B;

[0115] S4. Preparation of reactive internal plasticizing monomer resin emulsion

[0116] The remaining amount of deionized water is heated to 80° C., the remaining amount of emulsifier is added, 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution are added, and the mixture is stirred at a constant temperature for 20 minutes. Then, 50% by weight of the remaining monomer pre-emulsion A is added dropwise while stirring within 1 hour. After the reaction is completed, the whole amount of monomer pre-emulsion B is added dropwise while stirring within 1 hour. After the reaction is completed, the remaining weight of the monomer pre-emulsion A is added dropwise while stirring within 1 hour. After the addition is completed, the mixture is stirred at a constant temperature for 1 hour at 85° C. After the reaction is completed, the temperature of the reaction system is lowered to 65° C., and then the whole amount of the reducing agent solution is added dropwise while stirring, and the addition is completed within 1 hour. Then, the mixture is stirred at a constant temperature for 1 hour. Then, the temperature of the reaction system is lowered to room temperature, the remaining amount of the neutralizer is added, and the mixture is stirred for 0.5 hours. The reaction solution is filtered through a 240-mesh filter to obtain a reactive block plasticizer emulsion with a particle size range of 50-150 nm.

[0117] S5. Preparation of reactive internal plasticizing monomer resin powder

[0118] The reactive block plasticizer emulsion obtained in step S4 is subjected to high-speed centrifugation and spray drying to obtain a powder, i.e., a reactive block plasticizer having an ABA type hard segment-soft segment-hard segment block structure, wherein the A segment is an epoxy acrylate copolymer segment, and the B segment is an internal plasticizing monomer copolymer segment. The centrifugal speed is 18000 rpm, the spray drying inlet temperature is 160° C., and the outlet temperature is 90° C.

[0119] The modified PLA low-temperature shrink film is prepared by the following method:

[0120] Step 1, according to the formula amount, PLA, reactive block plasticizer, lubricant, and anti-aging agent are uniformly blended to obtain a mixed material, and then the mixed material is added to a twin-screw extruder, heated and melt-blended, and then extruded and cast through a die head of the twin-screw extruder to obtain a cast sheet;

[0121] Step 2, biaxially stretching the cast sheet obtained in step (1), first longitudinally stretching and then transversely stretching, and then heat-setting to obtain a modified PLA low-temperature shrink film.

[0122] In step (1), the blending stirring speed is 700 rpm, the blending time is 25 min, the melt blending temperature is 170° C., the temperature of the twin-screw extruder die head is 205° C., and the temperature of the casting roll is 40° C.

[0123] In step (2), the temperature of biaxial stretching is controlled at 55°C, the stretching speed is controlled at 60 mm / s, the stretching ratio is 4, and the heat setting temperature is 100°C.

[0124] Example 3

[0125] A modified PLA low-temperature shrink film, which has the following components in parts by weight:

[0126] PLA 700 copies;

[0127] 20 parts of reactive block plasticizer;

[0128] 2 parts of lubricant;

[0129] 0.5 parts of anti-aging agent.

[0130] The raw materials of the reactive block plasticizer are composed of the following in parts by weight:

[0131] 4 parts of emulsifier;

[0132] 130 parts of hard segment monomer;

[0133] Internal plasticizing monomer 170 parts;

[0134] 8 parts of functional monomer;

[0135] 5 parts of cross-linking monomer;

[0136] 1.8 parts of initiator;

[0137] 5 parts of neutralizer;

[0138] 0.8 part of reducing agent;

[0139] 300 parts of deionized water.

[0140] The lubricant is prepared by mixing erucamide and zinc stearate in a mass ratio of 1:1, and the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 1.5:1.

[0141] The emulsifier is prepared by mixing emulsifier Adeka REASOAP SR-10 and emulsifier DES-30 in a weight ratio of 1:2.

[0142] The hard segment monomer is a mixture of methyl methacrylate, styrene and glycidyl methacrylate in a weight ratio of 2:1:2.

[0143] The internal plasticizing monomer is a mixture of isooctyl acrylate and di-n-butyl itaconate in a weight ratio of 1:2.

[0144] The functional monomer is β-acryloxypropionic acid.

[0145] The cross-linking monomer is HDDA.

[0146] The initiator is potassium persulfate.

[0147] The neutralizing agent is aqueous ammonia.

[0148] The reducing agent is sodium benzenesulfinate.

[0149] The reactive block plasticizer is prepared by the following method:

[0150] S1, dissolving the formulated amount of initiator in 1 / 20 of the formulated amount of deionized water to obtain an initiator solution;

[0151] Adding a formula amount of reducing agent to 1 / 20 of the formula amount of deionized water to obtain a reducing agent solution;

[0152] S2. Preparation of monomer pre-emulsion A

[0153] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of hard segment monomer, 1 / 2 of the formula amount of cross-linking monomer, 1 / 2 of the formula amount of functional monomer, 1 / 3 of the formula amount of initiator solution, and 1 / 4 of the formula amount of neutralizer are sequentially added thereto, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion A;

[0154] S3, preparation of monomer pre-emulsion B

[0155] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of internal plasticizer monomer, the remaining formula amount of cross-linking monomer, the remaining formula amount of functional monomer, 1 / 3 weight part of initiator solution, and 1 / 4 weight part of neutralizer are added thereto in sequence, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion solution B;

[0156] S4. Preparation of reactive internal plasticizing monomer resin emulsion

[0157] The remaining amount of deionized water is heated to 80° C., the remaining amount of emulsifier is added, 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution are added, and the mixture is stirred at a constant temperature for 20 minutes. Then, 50% by weight of the monomer pre-emulsion A is added dropwise while stirring within 1.2 hours. After the reaction is completed, the whole amount of the monomer pre-emulsion B is added dropwise while stirring within 1 hour. After the reaction is completed, the remaining weight of the monomer pre-emulsion A is added dropwise while stirring within 1 hour. After the addition is completed, the mixture is stirred at a constant temperature for 1 hour at 85° C. After the reaction is completed, the temperature of the reaction system is lowered to 62° C. Then, the whole amount of the reducing agent solution is added dropwise while stirring, and the addition is completed within 1 hour. Then, the mixture is stirred at a constant temperature for 1 hour. Then, the temperature of the reaction system is lowered to room temperature. The remaining amount of the neutralizer is added, and the mixture is stirred for 0.5 hours. The reaction solution is filtered through a 240-mesh filter to obtain a reactive block plasticizer emulsion with a particle size range of 50-150 nm.

[0158] S5. Preparation of reactive internal plasticizing monomer resin powder

[0159] The reactive block plasticizer emulsion obtained in step S4 is subjected to high-speed centrifugation and spray drying to obtain a powder, i.e., a reactive block plasticizer having an ABA type hard segment-soft segment-hard segment block structure, wherein the A segment is an epoxy acrylate copolymer segment, and the B segment is an internal plasticizing monomer copolymer segment. The centrifugal speed is 18000 rpm, the spray drying inlet temperature is 150° C., and the outlet temperature is 85° C.

[0160] The modified PLA low-temperature shrink film is prepared by the following method:

[0161] Step 1, according to the formula amount, PLA, reactive block plasticizer, lubricant, and anti-aging agent are uniformly blended to obtain a mixed material, and then the mixed material is added to a twin-screw extruder, heated and melt-blended, and then extruded and cast through a die head of the twin-screw extruder to obtain a cast sheet;

[0162] Step 2, biaxially stretching the cast sheet obtained in step (1), first longitudinally stretching and then transversely stretching, and then heat-setting to obtain a modified PLA low-temperature shrink film.

[0163] In step (1), the blending stirring speed is 750 rpm, the blending time is 30 min, the melt blending temperature is 185° C., the temperature of the twin-screw extruder die head is 210° C., and the temperature of the casting roll is 45° C.

[0164] In step (2), the temperature of biaxial stretching is controlled at 60°C, the stretching speed is controlled at 80 mm / s, the stretching ratio is 4, and the heat setting temperature is 110°C.

[0165] Example 4

[0166] A modified PLA low-temperature shrink film, which has the following components in parts by weight:

[0167]

[0168] The raw materials of the reactive block plasticizer are composed of the following in parts by weight:

[0169]

[0170] The lubricant is prepared by mixing erucamide and zinc stearate in a mass ratio of 3:1, and the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 1.5:1.

[0171] The emulsifier is prepared by mixing emulsifier Adeka REASOAP SR-10 and emulsifier DES-30 in a weight ratio of 1:2.

[0172] The hard segment monomers are composed of methyl methacrylate, isobornyl methacrylate and methyl methacrylate in a mass ratio of 2:0.5:2.

[0173] The internal plasticizing monomer is a mixture of isooctyl acrylate and dibutyl fumarate in a weight ratio of 1:2.

[0174] The functional monomer is β-acryloxypropionic acid.

[0175] The cross-linking monomer is DEGDMA.

[0176] The initiator is potassium persulfate.

[0177] The neutralizing agent is ammonia water with a mass concentration of 20%.

[0178] The reducing agent is disodium glycolate sulfinate.

[0179] The reactive block plasticizer is prepared by the following method:

[0180] S1, dissolving the formulated amount of initiator in 1 / 20 of the formulated amount of deionized water to obtain an initiator solution;

[0181] Adding a formula amount of reducing agent to 1 / 20 of the formula amount of deionized water to obtain a reducing agent solution;

[0182] S2. Preparation of monomer pre-emulsion A

[0183] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of hard segment monomer, 1 / 2 of the formula amount of cross-linking monomer, 1 / 2 of the formula amount of functional monomer, 1 / 3 of the formula amount of initiator solution, and 1 / 4 of the formula amount of neutralizer are sequentially added thereto, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion A;

[0184] S3, preparation of monomer pre-emulsion B

[0185] 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of internal plasticizer monomer, the remaining formula amount of cross-linking monomer, the remaining formula amount of functional monomer, 1 / 3 weight part of initiator solution, and 1 / 4 weight part of neutralizer are added thereto in sequence, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion solution B;

[0186] S4. Preparation of reactive internal plasticizing monomer resin emulsion

[0187] Heat the remaining amount of deionized water to 80°C, add the remaining amount of emulsifier, add 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution, stir and react at constant temperature for 20 minutes, then add 50% by weight of the remaining monomer pre-emulsion A dropwise within 1.5 hours while stirring. After the reaction is completed, immediately add all of the monomer pre-emulsion B dropwise within 1.5 hours while stirring. After the reaction is completed, immediately add the remaining weight of the monomer pre-emulsion B dropwise within 1.5 hours while stirring. After the emulsion A is added, it is stirred at a constant temperature of 85°C for 1 hour. After the reaction is completed, the temperature of the reaction system is lowered to 65°C, and then all the reducing agent solution is continuously added while stirring, and the addition is completed within 1 hour. Then, the reaction is stirred at a constant temperature for 1 hour. After that, the temperature of the reaction system is lowered to room temperature, and the remaining amount of neutralizer is added. After stirring for 0.5 hours, the reaction solution is filtered with a 240-mesh filter to obtain a reactive block plasticizer emulsion with a particle size range of 50-150nm;

[0188] S5. Preparation of reactive internal plasticizing monomer resin powder

[0189] The reactive block plasticizer emulsion obtained in step S4 is subjected to high-speed centrifugation and spray drying to obtain a powder, i.e., a reactive block plasticizer having an ABA type hard segment-soft segment-hard segment block structure, wherein the A segment is an epoxy acrylate copolymer segment, and the B segment is an internal plasticizing monomer copolymer segment. The centrifugal speed is 18000 rpm, the spray drying inlet temperature is 160° C., and the outlet temperature is 80° C.

[0190] The modified PLA low-temperature shrink film is prepared by the following method:

[0191] Step 1, according to the formula amount, PLA, reactive block plasticizer, lubricant, and anti-aging agent are uniformly blended to obtain a mixed material, and then the mixed material is added to a twin-screw extruder, heated and melt-blended, and then extruded and cast through a die head of the twin-screw extruder to obtain a cast sheet;

[0192] Step 2, biaxially stretching the cast sheet obtained in step (1), first longitudinally stretching and then transversely stretching, and then heat-setting to obtain a modified PLA low-temperature shrink film.

[0193] In step (1), the blending stirring speed is 800 rpm, the blending time is 30 min, the melt blending temperature is 190° C., the temperature of the twin-screw extruder die head is 210° C., and the temperature of the casting roll is 55° C.

[0194] In step (2), the temperature of biaxial stretching is controlled at 70°C, the stretching speed is controlled at 100 mm / s, the stretching ratio is 6, and the heat setting temperature is 120°C.

[0195] Comparative Example 1 is the same as Example 1, except that the molecular structure of the hard segment monomer used in Comparative Example 1 does not contain an epoxy group, and Comparative Example 1 uses methyl methacrylate in equal parts by weight to replace the glycidyl acrylate in Example 1.

[0196] Comparative Example 2 is the same as Example 1, except that in Comparative Example 2, dimethyl itaconate is used in equal parts by weight to replace dioctyl maleate in Example 1.

[0197] Comparative Example 3 is the same as Example 1, except that step S4 in Comparative Example 3 is different from that in Example 1, and step S4 in Comparative Example 3 is specifically as follows:

[0198] The remaining amount of deionized water is heated to 80°C, the remaining amount of emulsifier is added, 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution are added, and the mixture is stirred at a constant temperature for 20 minutes. Then, the remaining monomer pre-emulsion A is added dropwise while stirring within 1.5 hours. After the reaction is completed, the whole monomer pre-emulsion B is added dropwise while stirring within 1.5 hours. After the addition is completed, the mixture is stirred at a constant temperature for 1 hour at 85°C. After the reaction is completed, the temperature of the reaction system is lowered to 60°C. Then, the whole reducing agent solution is added dropwise while stirring and the addition is completed within 1 hour. Then, the mixture is stirred at a constant temperature for 0.5 hours. Then, the temperature of the reaction system is lowered to room temperature, the remaining amount of neutralizer is added, and the mixture is stirred for 0.5 hours. The reaction solution is filtered with a 240-mesh filter to obtain a reactive block plasticizer emulsion with a particle size range of 50-150 nm.

[0199] Comparative Example 4 is the same as Example 1, except that the reactive block plasticizer in Example 1 is replaced by triethyl citrate (TEC) in an equal amount by weight in Comparative Example 4.

[0200] Comparative Example 5 is the same as Example 1, except that the reactive block plasticizer in Example 1 is replaced by acetyl tributyl citrate (ATBC) in equal parts by weight in Comparative Example 5.

[0201] Comparative Example 6 is the same as Example 1, except that the reactive block plasticizer in Example 1 is replaced by an equal amount of epoxy soybean oil by weight in Comparative Example 6.

[0202] Performance Testing

[0203] The low-temperature shrinkage films obtained in Examples 1-4 of the present invention and Comparative Examples 1-7 were respectively subjected to relevant performance tests, and the test results are shown in Table 1.

[0204] The tests of light transmittance and haze are carried out in accordance with GB / T 2410-2008, the test of shrinkage is carried out in accordance with GB / T 12027-2004, and the test of mechanical properties is carried out in accordance with GB / T 1040.2-2006.

[0205] Table 1

[0206]

[0207] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A reactive block plasticizer, characterized in that: The reaction raw materials include the following components in parts by weight: Emulsifier 2.4-5 parts; 120-150 parts of hard segment monomer; Internal plasticizing monomer 150-180 parts; 6-9 copies of functional monomer; 3-9 parts of cross-linking monomer; Initiator 1.5-2.1 parts; 3-6 parts of neutralizer; Reducing agent 0.5-0.8 parts; 250-300 parts of deionized water.

2. A reactive block plasticizer according to claim 1, characterized in that: The hard segment monomers include one or more of methyl methacrylate, styrene, isobornyl methacrylate, and glycidyl methacrylate.

3. A reactive block plasticizer according to claim 1, characterized in that: The internal plasticizing monomer includes one or more of di-n-butyl itaconate, dioctyl maleate, dibutyl fumarate, butyl acrylate, and isooctyl acrylate.

4. A reactive block plasticizer according to claim 1, characterized in that: The functional monomers include one or more of methacrylic acid, acrylic acid, and β-acryloxypropionic acid.

5. A reactive block plasticizer according to claim 1, characterized in that: The cross-linking monomer includes one or more of TPGDA, TMPTA, HDDA, and DEGDMA.

6. A reactive block plasticizer according to claim 1, characterized in that: The reducing agent is a sodium salt of an organic sulfinic acid derivative.

7. A reactive block plasticizer according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: S1, dissolving the formulated amount of initiator in 1 / 20 of the formulated amount of deionized water to obtain an initiator solution; Adding a formula amount of reducing agent to 1 / 20 of the formula amount of deionized water to obtain a reducing agent solution; S2. Preparation of monomer pre-emulsion A 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of hard segment monomer, 1 / 2 of the formula amount of cross-linking monomer, 1 / 2 of the formula amount of functional monomer, 1 / 3 of the formula amount of initiator solution, and 1 / 4 of the formula amount of neutralizer are sequentially added thereto, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion A; S3, preparation of monomer pre-emulsion B 45% of the formula amount of emulsifier and 1 / 3 of the formula amount of deionized water are mixed to obtain an emulsifier aqueous solution, and the formula amount of internal plasticizer monomer, the remaining formula amount of cross-linking monomer, the remaining formula amount of functional monomer, 1 / 3 weight part of initiator solution, and 1 / 4 weight part of neutralizer are added thereto in sequence, and the mixture is stirred and dispersed at room temperature for 30 minutes to prepare a monomer pre-emulsion solution B; S4. Preparation of reactive internal plasticizing monomer resin emulsion Heat the remaining amount of deionized water to 80°C, add the remaining amount of emulsifier, add 5% by weight of the monomer pre-emulsion A obtained in step (1) and the remaining weight of the initiator solution, stir and react at constant temperature for 20 minutes, then add 50% by weight of the remaining monomer pre-emulsion A dropwise while stirring within 0.5h-1.5h. After the reaction is completed, immediately add all of the monomer pre-emulsion B dropwise while stirring within 1h-1.5h. After the reaction is completed, immediately add the remaining weight of the monomer pre-emulsion B dropwise while stirring within 0.5h-1.5h. After the addition of monomer pre-emulsion A is completed, the mixture is stirred at a constant temperature of 85°C for 1 hour. After the reaction is completed, the temperature of the reaction system is lowered to 60-65°C. After that, the whole reducing agent solution is continuously added dropwise while stirring, and the addition is completed within 1 hour. After that, the mixture is stirred at a constant temperature for 0.5-1 hour. After that, the temperature of the reaction system is lowered to room temperature, and the remaining amount of neutralizer is added. After stirring for 0.5 hour, the reaction solution is filtered with a 240-mesh filter to obtain a reactive block plasticizer emulsion with an average particle size range of 50-150 nm. S5. Preparation of reactive internal plasticizing monomer resin powder The reactive block plasticizer emulsion obtained in step S4 is subjected to high-speed centrifugation and spray drying to be made into powder, thereby obtaining a reactive block plasticizer having an ABA type hard segment-soft segment-hard segment block structure, wherein the A segment is an epoxy acrylate copolymer segment, and the B segment is an internal plasticizer monomer copolymer segment.

8. A modified PLA low-temperature shrink film, characterized in that: The reactive block plasticizer according to any one of claims 1 to 6 is used as the plasticizer.

9. The modified PLA low-temperature shrink film according to claim 8, characterized in that: The composition includes the following components by weight: PLA 600-750 parts; 10-60 parts of reactive block plasticizer; 1-3 parts of lubricant; Anti-aging agent 0.5-1 part.

10. The modified PLA low-temperature shrink film according to claim 8, characterized in that: The preparation method comprises the following steps: Step 1, according to the formula amount, PLA, reactive block plasticizer, lubricant, and anti-aging agent are uniformly blended to obtain a mixed material, and then the mixed material is added to a twin-screw extruder, heated and melt-blended, and then extruded and cast through a die head of the twin-screw extruder to obtain a cast sheet; Step 2, biaxially stretching the cast sheet obtained in step (1), first longitudinally stretching and then transversely stretching, and then heat-setting to obtain a modified PLA low-temperature shrink film.