Fluorine-containing polyimide oligomer chain-extended polyurethane elastomer and preparation method thereof
Through fluorine-containing polyimide oligomer chain extension technology, the thermal stability, water resistance and irrepairability problems of polyurethane elastomers are solved, and high-strength, toughness and repairable polyurethane elastomers are prepared, which are suitable for a variety of applications. High performance applications.
Patent Information
- Application Number
- CN202410934263.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional polyurethane elastomers cannot be repaired or recycled when mechanically damaged, resulting in resource waste and environmental pollution. At the same time, their thermal stability, water resistance, and strength are insufficient, limiting their application scenarios.
A method for preparing polyurethane elastomers using fluorine-containing polyimide oligomer chain extension is used to synthesize prepolymers through imidization, prepare polyamic acid solutions, and perform primary and secondary chain extensions to form high-strength, repairable and reusable Recycled polyurethane elastomer uses multiple hydrogen bonds and fluorine elements to improve the material's mechanical properties and weather resistance.
It achieves the high strength, toughness, water resistance and self-healing properties of polyurethane elastomer, extends the service life of the material, and improves its thermal stability and recyclability. It is suitable for manufacturing impact-resistant protective coatings and electronic components.
Smart Images

Figure CN118725244A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane elastomer with a fluorinated polyimide oligomer chain extension and a preparation method thereof, belonging to the technical field of high-strength and tough polyurethane elastomers containing polyimide, and in particular to a preparation method of a fluorinated polyimide polymer, a repairable and recyclable high-performance elastomer based on multiple hydrogen bonds. Background Art
[0002] Polyurethane elastomers have been widely used in daily life and other fields due to their excellent mechanical properties and good processing properties. From traditional vehicle manufacturing and decoration building materials to emerging sensors, flexible robots, 3D printing, electronic skin and other fields, polyurethane elastomers are widely used. However, with the development of technology, people's requirements for materials are getting higher and higher, and the thermal stability, water resistance, strength and other properties of polyurethane elastomers limit their further application. In order to broaden the use scenarios of polyurethane elastomers, improving the mechanical stability, water resistance and thermal stability of polyurethane elastomer materials has always been the focus of research. In addition, traditional polyurethane elastomers cannot be repaired or recycled when they are mechanically damaged and can only be replaced, which causes waste of resources and environmental pollution. Requiring materials to have excellent self-healing and repeatable processing properties is a new research hotspot. Summary of the invention
[0003] The technical problem solved by the invention is: to overcome the deficiencies of the prior art and to provide a polyurethane elastomer with a fluorinated polyimide oligomer chain extension and a preparation method thereof.
[0004] The technical solution adopted by the present invention is as follows:
[0005] The general structural formula of a polyurethane elastomer with a fluorinated polyimide oligomer chain extension is as follows:
[0006]
[0007] Obtained by imidization, as follows:
[0008]
[0009] In the formula, A1 is a fluorinated diamine monomer, and the structural formula is:
[0010]
[0011] A2 is a fluorinated dianhydride monomer with the structural formula:
[0012]
[0013] A3 is a prepolymer after hydrazide chain extension, and its structural formula is:
[0014]
[0015] D1 in A3 is a diisocyanate monomer, and its structural formula is:
[0016]
[0017] D2 in A3 is polytetrahydrofuran polyol, polycaprolactone polyol, polycarbonate polyol or polyether polyol, and has the structural formula:
[0018]
[0019] Among them, the value range of n1 is 10-30; the value range of n2 is 10-35; the value range of n3 is 10-40; the value range of n4 is 10-40;
[0020] The structural formula of D3 in A3 is:
[0021] The value range of n is 2-8;
[0022] The value range of a is 5-30; the value range of b is 5-30;
[0023] A method for preparing a polyurethane elastomer with a fluorinated polyimide oligomer chain extension comprises the following steps:
[0024] (1) Synthesis of prepolymer: under nitrogen protection, dehydrated polyol, diisocyanate, catalyst and organic solvent are uniformly mixed, and stirred at 50-100° C. for 1-6 hours to obtain a prepolymer; wherein the molar ratio of polyol to diisocyanate is 1:2-10; the water content of the polyol is less than 0.05%; the amount of the catalyst is 0.01%-1% of the total mass of all raw materials, preferably 0.1wt%; (all raw materials include dehydrated polyol, diisocyanate, catalyst and organic solvent); the content of the organic solvent is 50%-150% of the mass of the polyol;
[0025] (2) Preparation of polyamic acid solution: A fluorinated diamine is stirred in an organic solvent at room temperature until dissolved, and then cooled to 0-8° C. in an ice bath to obtain a diamine solution having a concentration of 0.1-0.5 g / mL.
[0026] The fluorine-containing dianhydride and the organic solvent are uniformly mixed to obtain a dianhydride solution; the concentration of the dianhydride solution is 0.1-0.5 g / mL.
[0027] Slowly drop the dianhydride solution into the diamine solution, react in an ice bath for 0.5-2 hours, and then react at room temperature for 2-12 hours to obtain a polyamic acid solution; wherein the molar ratio of the fluorinated diamine to the fluorinated dianhydride is (1.05-2.1):1;
[0028] (3) primary chain extension: subjecting the prepolymer obtained in step (1) to a first chain extension with an amide-containing diamine, reacting at 10-100° C. for 0.5-48 h to obtain a primary chain-extended prepolymer; wherein the molar ratio of the NCO in the prepolymer to the amino group in the amide-containing diamine is 1:(0.1-0.9), preferably 1:(0.5-0.6);
[0029] (4) Secondary chain extension: adding the polyamic acid solution obtained in step (2) dropwise to the primary chain extension prepolymer obtained in step (3), reacting at 60-100° C. for 1-5 days, drying in an oven at 50-80° C. for 1-5 days, then drying in a vacuum at 60-90° C. for 2-6 hours, and then drying in a vacuum at 170-200° C. for 3-12 hours to obtain a polyurethane elastomer; wherein the molar ratio of the amino content in the polyamic acid solution to the isocyanate content in the primary chain extension prepolymer is 0.9-1.2.
[0030] In the step (1), the polyol mainly comprises at least one of polyether polyol, polyester polyol, polycarbonate polyol and polycaprolactone polyol;
[0031] In the step (1), the diisocyanate mainly includes at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), and hexamethylene diisocyanate (HDI). Preferably, the isocyanate is isophorone diisocyanate (IPDI).
[0032] In the step (1), the catalyst is dibutyltin dilaurate;
[0033] The organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethyl sulfoxide, ethyl acetate, dichloromethane, dichloroethane, chloroform, toluene, acetone, tetrahydrofuran, and methyltetrahydrofuran, preferably N,N-dimethylformamide or N,N-dimethylacetamide;
[0034] In the step (2), the fluorinated diamine is 2,2-bis(4-aminophenyl)hexafluoropropane (6FDAM), 3,3'-diamino-5,5'-bis(trifluoromethyl)biphenyl (3,3-TFMB), di(3-aminophenyl)-4-(trifluoromethyl)phenylphosphine oxide (mDA6FPPO), 1,4-bis(4-amino-2-trifluoromethylphenoxy)-benzene (6FAPB), 2,5-bis(4-amino-2-trifluoromethylphenoxy)-tert-butylbenzene (DNTBHQ-2TF), 4,4'-bis(4-amino-2-trifluoromethylphenoxy)-biphenyl (DNBP-2TF), 1,4-diamino At least one of -2,3,5,6-tetrafluorophenyl (4FPPD), 4,4'-diaminooctafluorobiphenyl (8FZB), 4,4'-diaminooctafluorodiphenyl ether (8FODB), 5-trifluoromethyl-1,3-diaminobenzene (TFMB), 5-trifluoromethoxy-1,3-diaminobenzene (TFMOB), 1,2,3,3,4,4-hexafluoro-1,2-bis[4-(amino)phenoxy]cyclobutane (P6FCB), 2,2-bis(trifluoromethyl)-4,4-diaminobiphenyl (TFDB), and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP);
[0035] In the step (2), the fluorine-containing dianhydride is at least one of 4,4'-(hexafluoroisopropyl)diphthalic dianhydride (6FDA), 2,3,6,7-tetracarboxylic acid-9,9-bis(trifluoromethyl)xanthene dianhydride (6FCDA), 1,4-bis(trifluoromethyl)-2,3,5,6-benzenetetracarboxylic dianhydride (P6FDA), 1,4-bis(3,4-dicarboxytrifluorophenoxy)tetrafluorophthalic dianhydride (10FEDA), 1,4-difluoropyromellitic dianhydride (PF2DA), and 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]hexafluoropropane dianhydride (BFDA);
[0036] In the step (3), the structural formula of the diamine containing an amide bond is:
[0037]
[0038] The invention discloses a high-toughness and recyclable polyurethane elastomer with a fluorine-containing polyimide oligomer chain extension, the tensile strength of which is 20-100 MPa and the elongation at break is 200-1000%.
[0039] The invention discloses a high-toughness and recyclable polyurethane elastomer with fluorinated polyimide oligomer chain extension, which can be dissolved in N,N-dimethylformamide or N,N-dimethylacetamide and cast again, or formed again through a hot pressing process, and the performance can be restored to 80-100% of the original sample; wherein the hot pressing process parameters include a pressure of 2-10MPa, a hot pressing temperature of 170-220°C, and a time of 5-30min.
[0040] The high-toughness and recyclable polyurethane elastomer prepared by the invention with chain extension of fluorinated polyimide oligomer can be used for manufacturing impact-resistant protective coatings, electronic components and electronic skin.
[0041] Beneficial Effects
[0042] (1) Through molecular structure design, the material is regulated from the microstructure, and the fluorinated polyimide and the polyurethane prepolymer are combined to realize the combination of the rigid segment of the high-rigidity nanostructure and the soft segment containing the non-covalent cross-linking part. The rigid polyimide can form a microphase separation structure reinforcement material, giving the elastomer excellent mechanical properties. The reversible breakage of a large number of hydrogen bonds in the flexible polyurethane segment under the action of external force can dissipate energy, improve the tensile strength and toughness of the material, and achieve the strength and toughness of the material.
[0043] (2) Fluorine is introduced into polyurethane elastomers. Due to the small atomic radius and high electronegativity of fluorine atoms, fluorine elements tend to migrate and enrich on the surface, making it have a very low surface tension, thus exhibiting excellent water resistance and stain resistance. At the same time, due to the small atomic radius of fluorine atoms, they can tightly wrap the carbon chain skeleton to produce a spatial shielding effect. This spatial shielding makes the molecular chain of polyurethane well protected by the surrounding fluorine atoms, and the polyurethane elastomer has excellent weather resistance and chemical stability.
[0044] (3) Using chain extenders containing amide bonds to introduce multiple hydrogen bonds into the polyurethane segments for synergistic effects, they serve as physical crosslinking points to form a strong three-dimensional crosslinked network. When the material is deformed, the opening of the hydrogen bonds and the stretching of the flexible polymer segments can increase energy dissipation, thereby giving the elastomer high toughness. In addition, hydrogen bonds are dynamically reversible, giving the material self-healing properties and repeatable processing properties. It is often difficult to combine high strength and repairable / recyclable properties of materials. It is a very challenging method to use a dynamic crosslinking strategy and use fluorinated polyimide oligomers to extend the chain to prepare high-strength, high thermal stability, and weather-resistant repairable / recyclable polyurethane elastomers.
[0045] Aiming to solve the problems of thermal stability, water resistance, low strength and non-reusability of existing polyurethane elastomers, starting from molecular structure design to enhance material performance, a high-performance fluorinated polyimide polyurethane elastomer based on multiple hydrogen bonds that is repairable and recyclable and a preparation method thereof are provided. The structure of the elastomer includes a soft segment elastic matrix cross-linked by reversible hydrogen bonds and a uniformly dispersed rigid fluorinated polyimide nanostructure. Not only does the introduction of multiple hydrogen bonds in the polyurethane hard segment give the polyurethane elastomer a repairable property, but it also greatly improves the strength and toughness of the elastomer.
[0046] In order to further improve the performance of traditional polyurethane elastomers, the present invention uses amino-terminated fluorinated polyimide oligomers to extend the hydrogen-rich polyurethane prepolymers, and integrates the performance of fluorinated polymers and the excellent mechanical, thermal, electrical insulation and corrosion resistance of polyimides into polyurethane elastomers. Rigid polyimides can self-assemble to form microphase separation structure reinforcement materials, while a large number of hydrogen bonds in the flexible polyurethane segments can dissipate energy during the stretching process, thereby improving the stretchability and toughness of the material. The introduction of fluorine elements can improve the weather resistance, chemical corrosion resistance, and hydrophobic and oleophobic properties of polyurethane. In addition, the introduction of a large number of non-covalent hydrogen bonds between molecules can make the elastomer have better self-repairing and recyclability.
[0047] Fluorine-containing groups are introduced into polyimide and then combined with polyurethane elastomer. The rigid segments of high-rigidity nanostructures are combined with soft segments containing non-covalent cross-linked parts. This not only gives the elastomer excellent mechanical properties, but also the reversible breakage of multiple hydrogen bonds under external forces can effectively dissipate energy and improve the toughness and repairability of the material.
[0048] The present invention relates to the field of preparation of high-strength and tough polyurethane elastomers with fluorinated polyimide oligomer chain extension, and in particular to a method for preparing high-strength and tough, repairable and recyclable polyurethane elastomers based on multiple hydrogen bonds and fluorinated polyimide chain extension. By adopting fluorinated polyamic acid and an amide bond-containing chain extender to jointly extend a polyurethane prepolymer, a polyurethane elastomer material with fluorinated rigid polyimide segments and multiple hydrogen bonds is obtained. The performance of fluorinated polymers and the excellent mechanical, thermal, electrical insulation and corrosion resistance of polyimides are integrated into polyurethane elastomers. Rigid polyimides can self-assemble to form microphase separation structure reinforcement materials, while a large number of hydrogen bonds in flexible polyurethane segments can dissipate energy during stretching, thereby improving the stretchability and toughness of the material. In addition, the introduction of a large number of non-covalent hydrogen bonds between molecules can make the elastomer have better self-repair and recyclability, thereby extending the service life and cycle of the elastomer. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 The stress-strain curves of the polyurethane elastomer samples prepared in Examples 1-5;
[0050] Figure 2 This is a physical picture of the polyurethane elastomer sample prepared in Example 1;
[0051] Figure 3 The water contact angle test of the polyurethane elastomer sample prepared in Example 1, (a) is a real picture, (b) shows that the contact angle is 140°;
[0052] Figure 4 This is a picture of the polyurethane elastomer sample prepared in Example 1 being repaired after fracture. DETAILED DESCRIPTION
[0053] The present invention is further described and elaborated in detail below in conjunction with specific embodiments, which should not be regarded as specific limitations of the present invention.
[0054] Example 1
[0055] (1) Synthesis of prepolymer: Under nitrogen protection, dehydrated polytetrahydrofuran diol (PTMG 2000) (6 g, 3 mmol), isophorone diisocyanate (1.33 g, 6 mmol), dibutyltin dilaurate (7 mg, 0.1 wt%) and 1.8 g N,N-dimethylacetamide (DMAc) were mixed uniformly and stirred at 80° C. for 3 h to obtain a prepolymer;
[0056] (2) Synthesis of polyamic acid: 2,2-bis(4-aminophenyl)hexafluoropropane (6FDAM) (8 g, 24 mmol) was stirred in 40 g DMAc at room temperature until dissolved, and then cooled to 0°C in an ice bath; 4,4'-(hexafluoroisopropyl)diphthalic anhydride (6FDA) (8.88 g, 20 mmol) was mixed with 60 g DMAc and slowly added dropwise to the 6FDAM solution, reacted in an ice bath for 1 h, and then reacted at room temperature for 3 h to obtain a polyamic acid solution;
[0057] (3) Primary chain extension: The prepolymer obtained in step 1 was subjected to a first chain extension with adipic acid dihydrazide (0.26 g, 1.5 mmol) and reacted at 80° C. for 2 h to obtain a primary chain extension prepolymer;
[0058] (4) Secondary chain extension: The polyamic acid solution (44 mL) synthesized in step 2 was added dropwise to the primary chain extension prepolymer obtained in step 3, reacted at 80°C for 3 days, dried in an oven at 60°C for 1 day, and then vacuum-treated at 80°C for 3 hours and then at 180°C for 4 hours to obtain a polyurethane elastomer sample.
[0059] Example 2
[0060] (1) Synthesis of prepolymer: Under nitrogen protection, dehydrated polytetrahydrofuran diol (PTMG 2000) (6 g, 3 mmol), isophorone diisocyanate (1.33 g, 6 mmol), dibutyltin dilaurate (7 mg, 0.1 wt%) and 1.8 g N,N-dimethylacetamide (DMAc) were mixed uniformly and stirred at 80° C. for 3 h to obtain a prepolymer;
[0061] (2) Synthesis of polyamic acid: 2,2-bis(4-aminophenyl)hexafluoropropane (6FDAM) (7.35 g, 22 mmol) was stirred in 30 g DMAc at room temperature until dissolved, and then cooled to 0°C in an ice bath; 4,4'-(hexafluoroisopropyl)diphthalic anhydride (6FDA) (8.88 g, 20 mmol) was mixed with 60 g DMAc and slowly added dropwise to the 6FDAM solution, reacted in an ice bath for 1 h, and then reacted at room temperature for 3 h to obtain a polyamic acid solution;
[0062] (3) Primary chain extension: The prepolymer obtained in step 1 was subjected to a first chain extension with malonic acid hydrazide (0.24 g, 1.8 mmol) and reacted at 80° C. for 2 h to obtain a primary chain extension prepolymer;
[0063] (4) Secondary chain extension: The polyamic acid solution (64 mL) synthesized in step 2 was added dropwise to the primary chain extension prepolymer obtained in step 3, reacted at 80°C for 3 days, dried in an oven at 60°C for 2 days, then vacuum-dried at 80°C for 4 hours, and then at 180°C for 4 hours to obtain a polyurethane elastomer sample.
[0064] Example 3
[0065] (1) Synthesis of prepolymer: Under nitrogen protection, dehydrated polytetrahydrofuran diol (PTMG 2000) (6 g, 3 mmol), diphenylmethane diisocyanate (1.5 g, 6 mmol), dibutyltin dilaurate (7 mg, 0.1 wt%) and 1.8 g N, N-dimethylacetamide (DMAc) were mixed uniformly, and stirred at 80° C. for 3 h to obtain a prepolymer;
[0066] (2) Synthesis of polyamic acid: 2,2-bis(4-aminophenyl)hexafluoropropane (6FDAM) (7.35 g, 22 mmol) was stirred in 30 g DMAc at room temperature until dissolved, and then cooled to 0°C in an ice bath; 4,4'-(hexafluoroisopropyl)diphthalic anhydride (6FDA) (8.88 g, 20 mmol) was mixed with 60 g DMAc and slowly added dropwise to the 6FDAM solution, reacted in an ice bath for 1 h, and then reacted at room temperature for 3 h to obtain a polyamic acid solution;
[0067] (3) Primary chain extension: The prepolymer obtained in step 1 was subjected to a first chain extension with adipic acid dihydrazide (0.31 g, 1.8 mmol) and reacted at 80° C. for 2 h to obtain a primary chain extension prepolymer;
[0068] (4) Secondary chain extension: The polyamic acid solution (64 mL) synthesized in step 2 was added dropwise to the primary chain extension prepolymer obtained in step 3, reacted at 80°C for 3 days, dried in an oven at 60°C for 2 days, and then vacuum-dried at 80°C for 3 hours and then at 180°C for 4 hours to obtain a polyurethane elastomer sample.
[0069] Example 4
[0070] (1) Synthesis of prepolymer: Under nitrogen protection, dehydrated polytetrahydrofuran diol (PTMG 2000) (6 g, 3 mmol), isophorone diisocyanate (1.33 g, 6 mmol), dibutyltin dilaurate (7 mg, 0.1 wt%) and 1.8 g N,N-dimethylacetamide (DMAc) were mixed uniformly and stirred at 80° C. for 3 h to obtain a prepolymer;
[0071] (2) Synthesis of polyamic acid: 2,2-bis(trifluoromethyl)-4,4-diaminobiphenyl (TFDB) (7.7 g, 24 mmol) was stirred in 40 g DMAc at room temperature until dissolved, and then cooled to 0°C in an ice bath; 4,4'-(hexafluoroisopropyl)diphthalic anhydride (6FDA) (8.88 g, 20 mmol) was mixed with 60 g DMAc and slowly added dropwise to the TFDB solution, reacted in an ice bath for 1 h, and then reacted at room temperature for 3 h to obtain a polyamic acid solution;
[0072] (3) Primary chain extension: The prepolymer obtained in step 1 was subjected to a first chain extension with adipic acid dihydrazide (0.31 g, 1.8 mmol) and reacted at 80° C. for 3 h to obtain a primary chain extension prepolymer;
[0073] (4) Secondary chain extension: The polyamic acid solution (35 mL) synthesized in step 2 was added dropwise to the primary chain extension prepolymer obtained in step 3, reacted at 80°C for 3 days, dried in an oven at 60°C for 2 days, and then vacuum-treated at 80°C for 3 hours and then at 180°C for 4 hours to obtain a polyurethane elastomer sample.
[0074] Example 5
[0075] (1) Synthesis of prepolymer: Under nitrogen protection, dehydrated polycaprolactone diol (Mn=2000) (6 g, 3 mmol), isophorone diisocyanate (1.33 g, 6 mmol), dibutyltin dilaurate (7 mg, 0.1 wt%) and 1.8 g N,N-dimethylacetamide (DMAc) were mixed uniformly and stirred at 80° C. for 3 h to obtain a prepolymer;
[0076] (2) Synthesis of polyamic acid: 2,2-bis(trifluoromethyl)-4,4-diaminobiphenyl (TFDB) (7 g, 22 mmol) was stirred in 40 g DMAc at room temperature until dissolved, and then cooled to 0°C in an ice bath; 4,4'-(hexafluoroisopropyl)diphthalic anhydride (6FDA) (8.88 g, 20 mmol) was mixed with 60 g DMAc and slowly added dropwise to the TFDB solution, reacted in an ice bath for 1 h, and then reacted at room temperature for 3 h to obtain a polyamic acid solution;
[0077] (3) Primary chain extension: The prepolymer obtained in step 1 was subjected to a first chain extension with oxalic acid dihydrazide (0.21 g, 1.8 mmol) and reacted at 80° C. for 3 h to obtain a primary chain extension prepolymer;
[0078] (4) Secondary chain extension: The polyamic acid solution (70 mL) synthesized in step 2 was added dropwise to the primary chain extension prepolymer obtained in step 3, reacted at 80°C for 3 days, dried in an oven at 60°C for 2 days, then vacuum-dried at 80°C for 4 hours, and then at 180°C for 4 hours to obtain a polyurethane elastomer sample.
[0079] The tensile strength test of the polyurethane elastomer samples prepared in Examples 1-5 was performed, and the test results are shown in Table 1:
[0080] Table 1 Test results of polyurethane elastomer samples prepared in Examples 1-5
[0081] sample Tensile strength(MPa) Elongation at break (%) Example 1 57 693 Example 2 67 885 Example 3 65 836 Example 4 78 951 Example 5 97 878
[0082] The polyurethane elastomer samples prepared in Examples 1-5 were subjected to stress-strain tests, and the obtained stress-strain curves are as follows: Figure 1 The data statistics are shown in Table 1, which shows that the obtained samples have excellent strength and toughness.
[0083] Figure 2 This is a real picture of the polyurethane elastomer sample prepared in Example 1. It can be seen from the figure that the sample is light yellow and transparent, and has good light transmittance.
[0084] Figure 3 This is a water contact angle test of the polyurethane elastomer sample prepared in Example 1. (a) is a real picture, and (b) shows that the contact angle is 140°, indicating that the material has excellent hydrophobic properties.
[0085] Figure 4 This is a repaired image of the polyurethane elastomer sample prepared in Example 1 after fracture. The fracture surface of the broken specimen was smeared with N,N-dimethylacetamide, and then placed in an oven at 80°C for 24 hours. The cut was restored to its original state, indicating that the sample prepared in the present invention has good self-healing properties and can be recycled and reused.
[0086] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyurethane elastomer with a fluorinated polyimide oligomer chain extension, characterized in that The structural formula of the polyurethane elastomer is: Wherein, A1 is a fluorine-containing diamine monomer, A2 is a fluorine-containing dianhydride monomer, A3 is a prepolymer after hydrazide chain extension, and the value of a ranges from 5 to 30.
2. The polyurethane elastomer of claim 1 wherein: The polyurethane elastomer is obtained by imidization, as follows:
3. The polyurethane elastomer with chain extension of fluorinated polyimide oligomer according to claim 1 or 2, characterized in that: The structural formula of A1 is:
4. The polyurethane elastomer of claim 3 wherein: The structural formula of A2 is:
5. The polyurethane elastomer with fluorinated polyimide oligomer chain extension according to claim 3, characterized in that: The structural formula of A3 is: D1 in A3 is a diisocyanate monomer, and its structural formula is: D2 in A3 is polytetramethylene glycol, polycaprolactone glycol, polycarbonate glycol or polyether glycol, and has the structural formula: Among them, the value range of n1 is 10-30; the value range of n2 is 10-35; the value range of n3 is 10-40; the value range of n4 is 10-40; The structural formula of D3 in A3 is: The value range of n is 2-8; The value range of b is 5-30.
6. A method for preparing a polyurethane elastomer with a fluorinated polyimide oligomer chain extension, characterized in that The following steps are involved: (1) Synthesizing a prepolymer: under nitrogen protection, uniformly mixing a dehydrated polyol, a diisocyanate, a catalyst and an organic solvent, stirring and reacting at 50-100° C. for 1-6 hours to obtain a prepolymer; wherein the molar ratio of the polyol to the diisocyanate is 1:2-10; the water content of the polyol is less than 0.05%; the amount of the catalyst is 0.01%-1% of the total mass of all raw materials, and all raw materials include the dehydrated polyol, the diisocyanate, the catalyst and the organic solvent; the content of the organic solvent is 50%-150% of the mass of the polyol; (2) preparing a polyamic acid solution: stirring a fluorinated diamine in an organic solvent at room temperature until dissolved, then cooling in an ice bath to 0-8°C to obtain a diamine solution, wherein the concentration of the diamine solution is 0.1-0.5 g / mL; uniformly mixing a fluorinated dianhydride with the organic solvent to obtain a dianhydride solution; the concentration of the dianhydride solution is 0.1-0.5 g / mL; slowly dropping the dianhydride solution into the diamine solution, reacting in an ice bath for 0.5-2 hours, and then reacting at room temperature for 2-12 hours to obtain a polyamic acid solution; wherein the molar ratio of the fluorinated diamine to the fluorinated dianhydride is (1.05-2.1):1; (3) primary chain extension: subjecting the prepolymer obtained in step (1) to a first chain extension with a diamine containing an amide bond, reacting at 10-100° C. for 0.5-48 h to obtain a primary chain extension prepolymer; wherein the molar ratio of the NCO mole in the prepolymer to the amino group in the diamine containing an amide bond is 1:(0.1-0.9); (4) Secondary chain extension: adding the polyamic acid solution obtained in step (2) dropwise to the primary chain extension prepolymer obtained in step (3), reacting at 60-100° C. for 1-5 days, drying in an oven at 50-80° C. for 1-5 days, then drying in a vacuum at 60-90° C. for 2-6 hours, and then drying in a vacuum at 170-200° C. for 3-12 hours to obtain a polyurethane elastomer; wherein the molar ratio of the amino content in the polyamic acid solution to the isocyanate content in the primary chain extension prepolymer is 0.9-1.
2.
7. The method for preparing a polyurethane elastomer with chain extension of a fluorinated polyimide oligomer according to claim 6, characterized in that: In the step (1), the polyol is at least one of polyether polyol, polyester polyol, polycarbonate polyol and polycaprolactone polyol; In the step (1), the diisocyanate is at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate; In the step (1), the catalyst is dibutyltin dilaurate; The organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethyl sulfoxide, ethyl acetate, dichloromethane, dichloroethane, chloroform, toluene, acetone, tetrahydrofuran, and methyltetrahydrofuran.
8. The method for preparing a polyurethane elastomer with chain extension of a fluorinated polyimide oligomer according to claim 6 or 7, characterized in that: In the step (2), the fluorinated diamine is 2,2-bis(4-aminophenyl)hexafluoropropane (6FDAM), 3,3'-diamino-5,5'-bis(trifluoromethyl)biphenyl (3,3-TFMB), di(3-aminophenyl)-4-(trifluoromethyl)phenylphosphine oxide (mDA6FPPO), 1,4-bis(4-amino-2-trifluoromethylphenoxy)-benzene (6FAPB), 2,5-bis(4-amino-2-trifluoromethylphenoxy)-tert-butylbenzene (DNTBHQ-2TF), 4,4'-bis(4-amino-2-trifluoromethylphenoxy)-biphenyl (DNBP-2TF), 1,4-diamino At least one of -2,3,5,6-tetrafluorophenyl (4FPPD), 4,4'-diaminooctafluorobiphenyl (8FZB), 4,4'-diaminooctafluorodiphenyl ether (8FODB), 5-trifluoromethyl-1,3-diaminobenzene (TFMB), 5-trifluoromethoxy-1,3-diaminobenzene (TFMOB), 1,2,3,3,4,4-hexafluoro-1,2-bis[4-(amino)phenoxy]cyclobutane (P6FCB), 2,2-bis(trifluoromethyl)-4,4-diaminobiphenyl (TFDB), and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP); In the step (2), the fluorine-containing dianhydride is at least one of 4,4'-(hexafluoroisopropyl)diphthalic dianhydride (6FDA), 2,3,6,7-tetracarboxylic acid-9,9-bis(trifluoromethyl)xanthene dianhydride (6FCDA), 1,4-bis(trifluoromethyl)-2,3,5,6-benzenetetracarboxylic dianhydride (P6FDA), 1,4-bis(3,4-dicarboxytrifluorophenoxy)tetrafluorophthalic dianhydride (10FEDA), 1,4-difluoropyromellitic dianhydride (PF2DA), and 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]hexafluoropropane dianhydride (BFDA).
9. The method for preparing a polyurethane elastomer with chain extension of a fluorinated polyimide oligomer according to claim 6, characterized in that: In the step (3), the structural formula of the diamine containing an amide bond is:
10. An application of a polyurethane elastomer with chain extension of a fluorinated polyimide oligomer, characterized in that: Used to manufacture impact-resistant protective coatings, electronic components or electronic skin.
Citation Information
Cited By
Polyurethane elastomer as well as preparation method and application thereof
CN119331199A
A polyurethane elastomer, its preparation and use
CN119331199B
High-strength yellow fluorescent polyurethane elastomer and preparation method thereof
CN120271785A
Heat-resistant self-repairing polyurethane elastic system and preparation method thereof
CN120289748A
A heat-resistant self-repairing polyurethane elastic system and preparation method thereof
CN120289748B