Polyether ketone ketone and preparation method thereof

By mixing at low temperature and controlling reaction conditions under nitrogen protection, combined with acidic protic solution quenching and multiple washing methods, the problem of insufficient molecular weight and purity of polyetherketoneketone in the electrophilic substitution method was solved, and high-performance polyether was obtained. Ketone, suitable for a variety of high performance applications.

CN118725260AActive Publication Date: 2024-10-01SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI

Patent Information

Application Number
CN202310336584.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

In the prior art, the molecular weight of polyetherketoneketone synthesized by electrophilic substitution is not high and the purity is not high enough, making it difficult to meet the requirements of high performance and biocompatibility.

Method used

Under nitrogen protection, mix terephthaloyl chloride and/or isophthaloyl chloride and diphenyl ether at low temperature, add anhydrous aluminum chloride, control the temperature and reaction time, and then add the end-capping agent and acidic protic solution for quenching Sterilize and wash, and obtain high-purity, high-molecular-weight polyetherketoneketone through multiple washings and drying.

Benefits of technology

It has achieved the synthesis of high molecular weight and high purity polyetherketoneketone, which has better thermal stability and molding processing performance and is suitable for military industry, machinery, medical equipment and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725260A_ABST
    Figure CN118725260A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: firstly adding paraphthaloyl chloride or isophthaloyl chloride and diphenyl ether, then performing low-temperature prepolymerization for a certain time under the condition of adding a catalyst anhydrous aluminum chloride, and then adding the rest diphenyl ether to complete a short-chain end capping reaction. By reducing the temperature in the initial reaction process at the earlier stage and adopting the washing reagent selection and reflux method at the later stage, the obtained high-molecular polymer polyether ketone ketone has high purity and high molecular weight. According to the present invention, the content of the catalyst aluminum contained in the PEKK is low, and the tested intrinsic viscosity (high molecular weight) and the tensile strength are high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a polyetherketoneketone and a preparation method thereof. Background Art

[0002] Polyetherketoneketone (PEKK) is an aromatic polymer with one ether bond and two ketone bond repeating units in the main chain. Its density is 1.28-1.31 g / cm 3 , melting point 300℃-375℃. Polyetherketoneketone (PEKK) is a special engineering plastic with excellent performance. It is a type of polyaryletherketone and a semi-crystalline polymer material. Its glass transition temperature (155℃~175℃) and melting temperature (305℃~375℃) can be controlled and adjusted according to the different monomer dosages. The chemical structure of the neatly arranged benzene rings, ether bonds, and ketone groups in its molecular structure gives the PEKK molecule highly stable chemical bond characteristics, making it have excellent properties such as high strength, high chemical resistance, and high continuous use temperature. It can be used in the aerospace field and many other wide-ranging industrial applications, including the preparation of thermoplastic composite materials. At the same time, it can also be used to prepare biomedical implant materials.

[0003] For in vivo use, polyaryletherketone (PAEK) materials must further meet the requirements of biocompatibility. Ideally, there should be no unreacted monomers, catalyst residues or other reaction components in the synthesized polymer, that is, high purity of the polymer is required to meet the requirements of biocompatibility. In fact, the polymer is mixed with impurities, which can also cause instability of the polymer melt during processing. This can be a serious problem during further processing and molding, because instability can lead to performance changes during the manufacturing process, which may affect the performance of the product during use. For applications with high structural and performance requirements, such as aerospace, this is very undesirable.

[0004] At present, there are two main methods for synthesizing PEKK: nucleophilic substitution and electrophilic substitution. Although nucleophilic substitution can produce polyetherketoneketone with good stability, the synthesis conditions of nucleophilic substitution reaction are high, which increases the production cost. The electrophilic substitution method has simple synthesis conditions, usually using low-temperature polymerization, and requires simple processes, making it easy to industrialize. However, the molecular weight of the polyetherketoneketone synthesized by electrophilic substitution is not high, and the purity is not enough.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] The object of the present invention is to provide a polyetherketoneketone and a preparation method thereof, which can overcome the technical problems in the prior art that the polyetherketoneketone synthesized by electrophilic substitution has a low molecular weight and insufficient purity.

[0007] To achieve the above object, an embodiment of the present invention provides a method for preparing polyetherketoneketone, comprising:

[0008] Under nitrogen protection, terephthaloyl chloride and / or isophthaloyl chloride, diphenyl ether and a polymer solvent are mixed and the temperature is controlled to be low at -20 to -5°C;

[0009] During the stirring process, anhydrous aluminum chloride is added, and the temperature is raised to 10° C. to 40° C. and stirred for 0.1 h to 1 h to obtain a first mixed solution;

[0010] Continue to add diphenyl ether to the first mixed solution, control the temperature at 25°C-40°C, and react for 0.1h-6h to obtain a second mixed solution;

[0011] Adding a capping agent and maintaining the temperature at 25° C. to 40° C. for 1 to 4 hours to obtain a mixture of polyetherketoneketone products;

[0012] The polyetherketoneketone product mixture is added to an ice acidic proton solution for quenching, and filtered to obtain a crude polyetherketoneketone solid;

[0013] Washing the crude polyetherketoneketone solid with alcohol and ketone detergents, and then washing the polyetherketoneketone solid with water to obtain a wet polyetherketoneketone solid;

[0014] The wet polyetherketoneketone solid is dried to obtain polyetherketoneketone.

[0015] In one or more embodiments of the present invention, in the first mixed solution, the mass ratio of terephthaloyl chloride and / or isophthaloyl chloride to diphenyl ether is 2.39:1-1.5:1.

[0016] In one or more embodiments of the present invention, in the second mixed solution, the ratio of terephthaloyl chloride and / or isophthaloyl chloride to diphenyl ether is 1.3:1-1:1.1.

[0017] In one or more embodiments of the present invention, the end-capping agent is diphenyl ether, benzoyl chloride or p-chlorobenzoyl chloride, and the mass of terephthaloyl chloride and / or isophthaloyl chloride and diphenyl ether in the second mixed solution is m, and the mass of the end-capping agent is less than or equal to 0.87m.

[0018] In one or more embodiments of the present invention, the polymer solvent is one or a mixture of two or more of o-dichlorobenzene, ethylene dichloride, and dichloromethane.

[0019] In one or more embodiments of the present invention, the mass ratio of the added amount of the anhydrous aluminum chloride to the diphenyl ether in the first mixed solution is 6:1-3:1.

[0020] In one or more embodiments of the present invention, the alcohol and ketone detergents are selected from methanol, ethanol, propanol or acetone.

[0021] In one or more embodiments of the present invention, the prepared polyetherketoneketone has an aluminum metal residue in the range of 0-50 ppm and a chloride ion content in the range of 0-100 ppm.

[0022] In one or more embodiments of the present invention, the temperature for drying the wet polyetherketoneketone solid is between 120°C and 180°C.

[0023] An embodiment of the present invention further provides a polyetherketoneketone, which is prepared by the method described.

[0024] Compared with the prior art, the synthesis conditions adopted in the present invention can well solve the problem of synthesizing a high-purity and high-molecular-weight polymer polyetherketoneketone by electrophilic substitution, and the obtained PEKK polymer has good thermal stability and can be processed into products by extrusion molding, injection molding, compression molding, etc. The molded materials can be used in military industry, machinery, ships, etc. due to their high purity, and can also meet the requirements of implants in medical devices for PEKK. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a scanning electron microscope image (SEM) of a powder sample according to one embodiment of the present invention;

[0026] Figure 2 FIG. 5 is a thermogravimetric analysis (TG) graph of a powder sample according to an embodiment of the present invention. DETAILED DESCRIPTION

[0027] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0028] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0029] A method for preparing polyetherketoneketone according to a preferred embodiment of the present invention comprises:

[0030] s1. Under nitrogen protection, add terephthaloyl chloride or / and isophthaloyl chloride, diphenyl ether and a mixed solution of a polymerization solvent into a reaction kettle, and keep the temperature of the mixture within the temperature range of -20 to -5°C; while stirring, slowly add anhydrous aluminum chloride to obtain a first mixed solution; and stir at 10°C to 40°C for 0.1h-1h.

[0031] s2. Add a predetermined amount of diphenyl ether to the first mixed solution, stir for 0.1 h-3 h to obtain a second mixed solution, and heat the second mixed solution to 25° C.-40° C. to react for 0.1 h-6 h.

[0032] s3. Add a predetermined amount of end-capping agent within a temperature range of 25°C to 40°C, and maintain the temperature for 1 to 4 hours to obtain a mixture of polyetherketoneketone products.

[0033] s4. Add the polyetherketoneketone product mixture obtained above into an icy acidic proton solution for quenching, and filter to obtain a crude polyetherketoneketone solid.

[0034] s5. Repeatedly reflux wash the crude polyetherketoneketone solid with methanol or other alcohol or ketone solution and acidic solution, and then wash the polyetherketoneketone solid with water to obtain a wet polyetherketoneketone solid.

[0035] s6. Dry the wet polyetherketoneketone solid under reduced pressure in a temperature range of 120° C. to 180° C. to obtain polyetherketoneketone PEKK.

[0036] In step s5, a method of repeated reflux washing with detergent is adopted. This method not only saves detergent, but also the detergent can be recycled in the industrial production of PEKK, and ensures that the residual impurities in PEKK are minimized.

[0037] In the prepared polyetherketoneketone, the residual aluminum metal content is within the range of 0-50 ppm, the chloride ion content is within the range of 0-100 ppm, and the residual volatile matter is less than 0.1%.

[0038] In an embodiment of the present invention, terephthaloyl chloride or isophthaloyl chloride and diphenyl ether are first added, and then anhydrous aluminum chloride is added as a catalyst, and prepolymerized at low temperature for a certain period of time, and then the remaining diphenyl ether is added to complete the short chain end-capping reaction. In the embodiment of the present invention, the polyetherketoneketone of the obtained polymer has high purity and high molecular weight by lowering the temperature in the initial reaction process in the early stage and adopting the washing reagent selection and reflux method in the later stage. This is manifested in that the content of catalyst aluminum contained in PEKK is lower, and the tested intrinsic viscosity is high (high molecular weight) and tensile strength is large.

[0039] Example 1

[0040] N2 was used as protective gas throughout the reaction process. In a 1L reactor, the stirring device was turned on, and then 8.51g of diphenyl ether, 20.3g of terephthaloyl chloride and 400ml of dichloromethane were slowly added respectively.

[0041] The temperature in the entire reactor was cooled to -15°C. After the temperature stabilized, 37.32 g of aluminum chloride was slowly added to the reactor. 30 minutes after the catalyst was added, the temperature of the reactor was raised to 30°C.

[0042] After the reaction was continued for 1 hour, 8.51 g of diphenyl ether was added to the reactor, and the temperature was maintained at 30° C. for 3 hours.

[0043] Then, 0.01 g of benzoyl chloride was added into the reactor and the reaction was continued at 30° C. for 4 h.

[0044] Add 400 g of 4% hydrochloric acid aqueous solution on ice into the reaction system while keeping the temperature in the system below 30°C and stir for 30 minutes. After completion, perform solid-liquid separation by centrifugation, collect the solid, wash it with water several times, reflux it with ethanol once, wash it with water again, and dry it under reduced pressure at 150°C for 5 hours to obtain a polyetherketoneketone polymer.

[0045] The intrinsic viscosity in 96% sulfuric acid according to ISO 307 is 0.92 dL / g.

[0046] The obtained powder sample was molded into a test specimen by molding according to ISO 527 standard, and its tensile strength was tested, and the result was 128 MPa.

[0047] Through ICP testing, the aluminum ion content in the powder sample is 41PPM.

[0048] The scanning electron microscope (SEM) images of the powder samples obtained were Figure 1 As shown in the figure, the thermogravimetric analysis (TG) of the powder sample obtained is shown in the figure. Figure 2 shown.

[0049] Example 2

[0050] N2 was used as protective gas throughout the reaction process. In a 1L reactor, the stirring device was turned on, and then 8.51g of diphenyl ether, 13.7g of terephthaloyl chloride and 400ml of dichloromethane were slowly added respectively.

[0051] The temperature in the entire reactor was cooled to -15°C. After the temperature stabilized, 32 g of aluminum chloride was slowly added to the reactor. 30 minutes after the catalyst was added, the temperature of the reactor was raised to 30°C.

[0052] After the reaction was continued for 1 hour, 4.7 g of diphenyl ether was added to the reactor and the temperature was maintained at 30° C. for 2 hours.

[0053] Then, 0.01 g of benzoyl chloride was added into the reactor and the reaction was continued at 30° C. for 4 h.

[0054] Add 400 g of 4% hydrochloric acid aqueous solution on ice into the reaction system while keeping the temperature in the system below 30°C and stir for 30 minutes. After completion, perform solid-liquid separation by centrifugation, collect the solid, wash it with water several times, reflux it with ethanol once, wash it with water again, and dry it under reduced pressure at 150°C for 5 hours to obtain a polyetherketoneketone polymer.

[0055] The intrinsic viscosity in 96% sulfuric acid according to ISO 307 is 0.82 dL / g.

[0056] The obtained powder sample was molded into a test specimen by molding according to ISO 527 standard, and its tensile strength was tested, and the result was 105 MPa.

[0057] Through ICP testing, the aluminum ion content in the powder sample is 40PPM.

[0058] Example 3

[0059] N2 was used as protective gas throughout the reaction process. In a 1L reactor, the stirring device was turned on, and then 8.51g of diphenyl ether, 20.3g of terephthaloyl chloride and 400ml of dichloromethane were slowly added respectively.

[0060] The temperature in the entire reactor was cooled to -10°C. After the temperature stabilized, 37.32 g of aluminum chloride was slowly added to the reactor. 30 minutes after the catalyst was added, the temperature of the reactor was raised to 40°C.

[0061] After the reaction was continued for 1 hour, 8.51 g of diphenyl ether was added to the reactor, and the temperature was maintained at 30° C. for 3 hours.

[0062] Then, 0.01 g of chlorobenzoyl chloride was added into the reactor and the reaction was continued at 30° C. for 4 h.

[0063] Add 400 g of 4% hydrochloric acid aqueous solution on ice into the reaction system while keeping the temperature in the system below 30°C and stir for 30 minutes. After completion, perform solid-liquid separation by centrifugation, collect the solid, wash it with water several times, reflux it with ethanol once, wash it with water again, and dry it under reduced pressure at 150°C for 5 hours to obtain a polyetherketoneketone polymer.

[0064] The intrinsic viscosity in 96% sulfuric acid according to ISO 307 is 0.88 dL / g.

[0065] The obtained powder sample was molded into a test specimen by molding according to ISO 527 standard, and its tensile strength was tested, and the result was 110 MPa.

[0066] Through ICP testing, the aluminum ion content in the powder sample is 32PPM.

[0067] Example 4

[0068] N2 was used as protective gas throughout the reaction process. In a 1L reactor, the stirring device was turned on, and then 8.51g of diphenyl ether, 20.3g of terephthaloyl chloride and 400ml of dichloromethane were slowly added respectively.

[0069] The temperature in the entire reactor was cooled to -20°C. After the temperature stabilized, 37.32 g of aluminum chloride was slowly added to the reactor. 30 minutes after the catalyst was added, the temperature of the reactor was raised to 30°C.

[0070] After the reaction was continued for 1 hour, 8.51 g of diphenyl ether was added to the reactor, and the temperature was maintained at 20° C. for 3 hours.

[0071] Then, 0.01 g of benzoyl chloride was added into the reactor and the reaction was continued at 30° C. for 1 h.

[0072] Add 400 g of 4% hydrochloric acid aqueous solution on ice into the reaction system while keeping the temperature in the system below 30°C and stir for 30 minutes. After completion, perform solid-liquid separation by centrifugation, collect the solid, wash it with water several times, reflux it with methanol and ethanol once, wash it with water again, and dry it under reduced pressure at 150°C for 5 hours to obtain a polyetherketoneketone polymer.

[0073] The intrinsic viscosity in 96% sulfuric acid according to ISO 307 is 0.90 L / g.

[0074] The obtained powder sample was molded into a test specimen by molding according to ISO 527 standard, and its tensile strength was tested, and the result was 112 MPa.

[0075] Through ICP testing, the aluminum ion content in the powder sample is 25PPM.

[0076] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for preparing polyetherketoneketone, characterized in that: include: Under nitrogen protection, terephthaloyl chloride and / or isophthaloyl chloride, diphenyl ether and a polymer solvent are mixed and the temperature is controlled to be low at -20 to -5°C; During the stirring process, anhydrous aluminum chloride is added, and the temperature is raised to 10° C. to 40° C. and stirred for 0.1 h to 1 h to obtain a first mixed solution; Continue to add diphenyl ether to the first mixed solution, control the temperature at 25°C-40°C, and react for 0.1h-6h to obtain a second mixed solution; Adding a capping agent and maintaining the temperature at 25° C. to 40° C. for 1 to 4 hours to obtain a mixture of polyetherketoneketone products; The polyetherketoneketone product mixture is added to an ice acidic proton solution for quenching, and filtered to obtain a crude polyetherketoneketone solid; Washing the crude polyetherketoneketone solid with alcohol and ketone detergents, and then washing the polyetherketoneketone solid with water to obtain a wet polyetherketoneketone solid; The wet polyetherketoneketone solid is dried to obtain polyetherketoneketone.

2. The method for preparing polyetherketoneketone according to claim 1, characterized in that: In the first mixed solution, the mass ratio of terephthaloyl chloride and / or isophthaloyl chloride to diphenyl ether is 2.39:1-1.5:

1.

3. The method for preparing polyetherketoneketone according to claim 1, characterized in that: In the second mixed solution, the ratio of terephthaloyl chloride and / or isophthaloyl chloride to diphenyl ether is 1.3:1-1:1.

1.

4. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The end-capping agent is diphenyl ether, benzoyl chloride or p-chlorobenzoyl chloride, Taking the mass of terephthaloyl chloride and / or isophthaloyl chloride and diphenyl ether in the second mixed solution as m, the mass of the end-capping agent is less than or equal to 0.87m.

5. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The polymer solvent is one of o-dichlorobenzene, ethylene dichloride and dichloromethane or a mixture of two or more thereof.

6. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The mass ratio of the added amount of the anhydrous aluminum chloride to the diphenyl ether in the first mixed solution is 6:1-3:

1.

7. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The alcohol and ketone detergents are selected from methanol, ethanol, propanol or acetone.

8. The method for preparing polyetherketoneketone according to claim 1, characterized in that: In the prepared polyetherketoneketone, the residual aluminum metal content is within the range of 0-50ppm, and the chloride ion content is within the range of 0-100ppm.

9. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The drying temperature of wet polyetherketoneketone solid is 120°C-180°C.

10. A polyetherketoneketone, characterized in that The polyetherketoneketone is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of polyether ketone ketone resin

    CN114560998A

  • Polyether ketone ketone as well as preparation method and application thereof

    CN114805758A

  • Method for preparing polyaryletherketone resin by adopting heterogeneous suspension polymerization mechanism and polyaryletherketone resin

    CN115057993A

Cited By

  • High-strength polyetherketoneketone polymer and preparation method thereof

    CN120025538A

  • Process for the production of a polyetherketoneketone and its use

    CN121343136B