A quantum dot coated reflective film and preparation method thereof
The problem of poor stability of the quantum dot film is solved by mesoporous strontium-doped hydroxyapatite nanorods loaded with quantum dots and ceria-coated silane microspheres, and high brightness and wide color are achieved The optical reflective film in the domain meets the needs of high-quality display and simplifies the process flow.
Patent Information
- Application Number
- CN202411210531.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing quantum dot reflective films are prone to lose stability during the process, and the color purity and color gamut of traditional LCD backlights are limited, making it difficult to meet the needs of high-quality display.
Mesoporous strontium doped hydroxyapatite (SrHAp) nanorods are used to load quantum dot materials and combine with silica microspheres coated with ceria and vinyl trimethoxysilane to form quantum dispensing water The composition is coated on the PET base film by solvent-free ultraviolet curing method to form a reflective film.
It improves the stability of quantum dot materials and the brightness of light sources, enhances the color gamut and brightness, and has a simple and efficient process and is environmentally friendly.
Smart Images

Figure CN118725381B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical films, and in particular relates to a quantum dot coated reflective film and a preparation method thereof. Background Art
[0002] Liquid Crystal Display (LCD) has stable performance, long life and low cost, and has been widely used in various fields. The backlight source of traditional LCD display uses blue light LED to excite phosphor to emit white light, and its color purity and color gamut have great limitations, making it increasingly difficult to meet the needs of high-quality display.
[0003] The narrow emission characteristics of quantum dots can improve the color gamut of the film and show brighter colors. In the field of LCD display, quantum dots (PQDs) are generally used in the backlight module of LCD in the form of quantum dot films. However, quantum dots have a very large specific surface area, and their unique surface effects make them very sensitive to water vapor and oxygen. In polymer substrates, quantum dot materials are unstable, difficult to disperse, and easily quenched and deactivated, which further limits their application in optical film materials.
[0004] For example, invention patent CN 117930545A discloses a quantum dot reflective film and its preparation method, and a backlight module, which mainly loads quantum dots on mesoporous silica, applies it to the film material of the reflective film, embeds the quantum dots in the resin layer of the film material, and wraps PQDs@SiO2 again through bubbles. The bubbles contain inert gas, forming a unique structure of bubbles embedded in the resin and bubbles wrapping PQDs@SiO2, thereby solving the technical problem of poor stability of the quantum dot film. However, this structure is not easy to implement in terms of technology. The reflective film is mainly obtained by biaxial stretching, and it is difficult to achieve an inert gas atmosphere in the full process production line. Therefore, the PQDs material is very likely to have lost its stability during the stretching preparation process of the film material. Invention patent CN 114637061 A discloses a high-toughness and high-brightness reflective film and its preparation method. In order to solve the problems of the reflective sheet of the backlight module scratching the light guide plate and the reflective film being assembled into the backlight module and the low brightness, a thin film adhesive layer containing quantum dots is coated on the surface of the reflective film by a coating method; the adhesive layer can protect the reflective film from scratches and improve the toughness; the quantum dot material contained in the adhesive layer can improve the brightness of the light source, so that the reflective film has the performance of high toughness and high brightness. However, the direct addition of PQDs material to prepare the coating liquid makes the obtained quantum dot coated reflective film have poor stability and poor aging resistance. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a quantum dot coated reflective film and a preparation method thereof. The present invention uses mesoporous strontium doped hydroxyapatite (SrHAp) nanorod loaded quantum dots (CsPbBr3@SrHAp) material to enhance the stability of quantum dots in an organic system, and adds it together with silica microsphere particles double-coated with cerium dioxide (CeO2) and vinyltrimethoxysilane (VTMS) to prepare a quantum dot glue composition coating liquid, and the composition coating liquid is coated on a PET base film to prepare an optical reflective film, in order to obtain a high-brightness reflective film with good stability, wider overall light source color rendering, and higher color gamut.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0007] In one aspect, the present invention provides a quantum dot coated reflective film, comprising a substrate, and a quantum dot glue layer formed by coating and curing a quantum dot glue composition and disposed on one or more surfaces of the substrate.
[0008] Preferably, the thickness of the quantum dot glue layer is 2 to 18 μm.
[0009] Furthermore, the substrate is selected from one of polyethylene terephthalate, polymethyl methacrylate, polyethylene terephthalate-1,4-cyclohexanedimethanol, polycarbonate, polyamide, and polystyrene;
[0010] Preferably, the substrate is a PET reflective film substrate.
[0011] The quantum dot glue composition comprises resin glue, optical particles and additives;
[0012] The resin glue is a mixture of tripropylene glycol diacrylate and polyurethane acrylate, and the usage ratio of tripropylene glycol diacrylate to polyurethane acrylate is 1:2.9-3.8 in parts by mass.
[0013] The optical particles are light diffusion particles and quantum dot particles.
[0014] Preferably, the quantum dot glue composition comprises the following components:
[0015] Tripropylene glycol diacrylate 20-26 parts
[0016] Polyurethane acrylate 74-76 parts
[0017] Photoinitiator 184 1~3 parts
[0018] 4-12 parts of quantum dot particles
[0019] 1 to 3 parts of light diffusion particles
[0020] Furthermore, the light diffusion particles are silica nanoparticle microspheres coated with a double layer of cerium dioxide (CeO2) and vinyltrimethoxysilane (VTMS), which are denoted as SiO2@CeO2 / poly(VTMS) microspheres;
[0021] Preferably, the silicon dioxide nanoparticles have an average particle size of 100 to 150 nm and a purity of ≥ 99.9 wt%.
[0022] Furthermore, the SiO2@CeO2 / poly(VTMS) microspheres are prepared by the following steps:
[0023] Step 1: Preparation of SiO2@CeO2 microspheres: SiO2@CeO2 microspheres were prepared by homogeneous in situ precipitation method.
[0024] The specific steps are as follows: the silica microspheres are ultrasonically dispersed in a mixed solution of water and ethanol (the volume ratio of water to ethanol is 1:1) to prepare a 0.2wt% dispersion, Ce(NO3)3·6H2O and hexamethylenetetramine (HMT) are added in sequence, wherein the amount of Ce(NO3)3·6H2O to HMT is 3:2 by mass ratio; then the temperature of the mixture is raised to 70 ℃ and kept under reflux for 4h, and then cooled to room temperature. The product is purified by centrifugation (8000 rpm and 5 min), washed three times with water and dried at 60 ℃ to obtain CeO2@SiO2 microspheres.
[0025] Step 2, preparation of SiO2@CeO2 / poly(VTMS) double-layer microspheres: SiO2@CeO2 / poly(VTMS) double-layer microspheres were prepared by hydrothermal method.
[0026] The specific steps are as follows:
[0027] The SiO2@CeO2 microspheres prepared in step 1 were mixed with deionized water (the amount of SiO2@CeO2 microspheres and deionized water was m SiO2@CeO2 / V 去离子水 =1g / 70mL) was ultrasonically dispersed for 1 h; urea and sodium tartrate dihydrate (Na2C4H4O6·2H2O) were added in sequence (by mass, the ratio of SiO2@CeO2 microspheres to Na2C4H4O6·2H2O to urea was 1:21:4), and the suspension was mechanically stirred for 0.5 h; then vinyl trimethoxysilane (VTMS) was added (the amount of SiO2@CeO2 microspheres to VTMS was m SiO2@CeO2 / V VTMS=1g / 2 mL), and the pH value of the solution was adjusted to 3-4 with 1 M HCl solution. After stirring for 1 h, the mixed solution was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, sealed and maintained at 180 °C for 3 h. After the temperature was cooled, the reaction mixture was centrifuged at 8500 rpm for 5 minutes, the product was collected, and washed three times with deionized water. The final product was obtained after drying at 80 °C overnight.
[0028] The quantum dot particles are mesoporous SrHAp nanorods loaded with CsPbBr3 quantum dots, denoted as CsPbBr3@SrHAp nanorods;
[0029] Preferably, the mesoporous SrHAp nanorods are strontium-doped hydroxyapatite, prepared by a hydrothermal method according to a Ca / P and (Ca + Sr) / P molar ratio of 1.67;
[0030] Furthermore, the Sr in the mesoporous SrHAp nanorods 2 + / (Ca 2 + + Sr 2+ ) The molar ratios may be 0, 0.01, 0.03, 0.05, 0.07, 0.09, 0.10, 0.15 and 0.20 respectively;
[0031] Preferably, the Sr in the mesoporous SrHAp nanorods 2 + / (Ca 2 + + Sr 2+ ) The molar ratios can be 0.10 and 0.15 respectively.
[0032] Preferably, the mesoporous SrHAp nanorods have a length of 120-150 nm, a diameter of about 20 nm, and a mesoporous structure diameter of 5-15 nm.
[0033] Preferably, the particle size of the CsPbBr3 PQDs is 1 to 10 nm.
[0034] Furthermore, the mesoporous SrHAp nanorods are obtained by the following steps:
[0035] First, Na2HPO4·12 H2O was dissolved in deionized water to form a solution (labeled as solution-1), and 1 mol / L NaOH solution was added to adjust the pH value of solution-1 to 11.5; then an aqueous solution (labeled as solution-2) was prepared by dissolving Ca(NO3)2·4H2O and Sr(NO3)2 in 30 mL of deionized water and slowly added to solution-1 under magnetic stirring. Subsequently, the obtained white milky suspension was transferred to a polytetrafluoroethylene-lined stainless steel autoclave (100 mL capacity), sealed, and kept at 200 °C for 8 h; finally, under the condition of natural cooling of the autoclave, the precipitate was separated, washed with deionized water and ethanol in sequence, and the obtained powder was dried at 100 °C for 6 h.
[0036] Furthermore, the CsPbBr3@SrHAp is obtained by the following steps:
[0037] Step 1, preparation of CsPbBr3 PQDs solution: take a certain amount of CsPbBr3 PQDs, disperse the CsPbBr3 PQDs into a n-hexane solution to form a CsPbBr3 PQDs solution, wherein the concentration of PQDs is 5 to 30 wt%.
[0038] Step 2, preparation of CsPbBr3@SrHAp: a certain amount of SrHAp sample was added to the n-hexane solution and stirred, and then the CsPbBr3 PQDs solution obtained in step 1 was injected into the n-hexane solution. The amount of SrHAp sample and n-hexane was m / s. SrHAp / V 正己烷 =1g / 100mL. SrHAp and CsPbBr3 PQDs were fully mixed by stirring for 60-70min. The complex was separated by centrifugation at 4000rpm and washed twice with n-hexane. Finally, the CsPbBr3@SrHAp nanocomposite was obtained by drying in a vacuum oven for 1h.
[0039] The feasible synthesis mechanism of CsPbBr3@SrHAp nanocomposites is as follows: when CsPbBr3 PQDs solution is mixed with SrHAp powder, Pb 2+ Adsorbed on the surface of SrHAp, Br - Around Pb 2+ The ions aggregate to form an octahedral structure. Then, under continuous stirring, Cs + The ions gather around the octahedron electrostatically and adsorb on the SrHAp surface, causing the CsPbBr3 crystals to nucleate rapidly.
[0040] Furthermore, the auxiliary agent includes a photoinitiator.
[0041] Preferably, the photoinitiator includes photoinitiator 184 .
[0042] Preferably, the photoinitiator accounts for 1 to 3% of the weight of the resin glue.
[0043] Furthermore, the optical particles account for 5-15% of the weight of the resin glue.
[0044] Preferably, the quantum dot particles account for 60-90% of the weight of the optical particles.
[0045] In a second aspect, the present invention provides a method for preparing a quantum dot-coated reflective film, comprising the following steps:
[0046] Step 1, preparation of a quantum dot glue composition coating liquid, according to the above formula, placing each raw material in a closed container in the dark and magnetically stirring at room temperature, the stirring speed is 50 to 200 rpm, the stirring time is 5 to 30 min, and after stirring evenly, a quantum dot glue composition coating liquid is obtained;
[0047] Step 2: Coat the quantum dot glue composition coating liquid on one or both sides of the PET reflective base film, then place the film in a 100 W UV lamp (365 nm) for 10 minutes on each side, and finally bake it in an oven at 60 ° C for 24 hours to obtain a quantum dot coated reflective film based on the quantum dot glue composition.
[0048] Beneficial effects of the invention: The invention provides a quantum dot coated reflective film and a preparation method thereof. Compared with the prior art, the quantum dot reflective film provided by the invention comprises a reflective layer and an adhesive layer. The reflective layer has a high reflectivity, thereby improving the brightness; the adhesive layer can protect the reflective film from scratches and improve toughness; the adhesive layer contains quantum dot materials, which can improve the brightness of the light source, and is prepared by a solvent-free ultraviolet curing method, which is simple in process and more efficient and environmentally friendly.
[0049] Secondly, the quantum dot material is CsPbBr3, and it is loaded by mesoporous SrHAp nanorods. On the one hand, the SrHAp surface contains a large amount of -OH, which not only makes the surface carry negative charge, but also lays the foundation for the adsorption of heavy metal ions. On the other hand, the electrostatic adsorption of heavy metals by SrHAp is the most common adsorption mechanism. The introduction of Sr can effectively improve the adsorption capacity of hydroxyapatite for quantum dots. In summary, the surface of SrHAp nanorods with mesoporous structure and a large amount of negative charge is conducive to the adsorption of heavy metal ions and the active nucleation of CsPbBr3 PQDs. The surface of PQDs is modified by this inorganic matrix material, which not only improves the luminescence performance of PQDs, but also improves the stability of PQDs.
[0050] In addition, the introduction of light diffusion particles SiO2@CeO2 / poly(VTMS) synergistically with the quantum dot material improves the light output uniformity of the quantum dot reflective film.
[0051] Finally, the SrHAp nanorods loaded with quantum dots have a rod-like structure. On the one hand, the nanorods with abundant surface hydroxyl groups and a large aspect ratio can be evenly dispersed in the adhesive coating liquid through intramolecular or intermolecular interactions, alleviating the aggregation and sedimentation of polymer particles, which is beneficial to the dispersion of quantum dot materials. In addition, the diffusion particles are spherical structures, and the combination of multi-morphology particles forms a multi-morphology particle adhesive layer with a network structure, which can make the polymer particles more evenly distributed, and further improve the mechanical strength and scratch resistance of the reflective film, and promote the adaptability of the reflective film and the light guide plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 Schematic diagram of the structure of quantum dot CsPbBr3@SrHAp nanorods.
[0053] Figure 2 Schematic diagram of the structure of light-diffusing particles SiO2@CeO2 / poly(VTMS) double-layer microspheres.
[0054] Figure 3 Schematic diagram of the structure of the optical reflective film prepared by applying the adhesive layer composition based on quantum dot CsPbBr3@SrHAp nanorods and light diffusion particle SiO2@CeO2 / poly(VTMS) double-layer microspheres to the base film.
[0055] Figure 4 Schematic diagram of the structure of the optical reflective film prepared by applying the adhesive layer composition based on quantum dot CsPbBr3@SiO2 microspheres and light diffusion particle SiO2@CeO2 / poly (VTMS) double-layer microspheres to the base film.
[0056] 1——CsPbBr3 quantum dots; 2——mesoporous SrHAp nanorods; 3——SiO2 nanospheres; 4——CeO2 deposition layer; 5——poly(VTMS) layer; 6——quantum dot adhesive layer based on CsPbBr3@SrHAp; 7——reflective film substrate; 8——diffusive particles; 9——quantum dots; 10——quantum dot adhesive layer based on CsPbBr3@SiO2. DETAILED DESCRIPTION
[0057] The present invention is further described below in conjunction with specific implementation methods.
[0058] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are conventional methods in the art.
[0059] The SiO2@CeO2 / poly(VTMS) double-layer microspheres have a structure as shown in the attached Figure 2 As shown, it is prepared by the following steps:
[0060] The silicon dioxide nanoparticles have an average particle size of 100 to 150 nm and a purity of ≥ 99.9 wt %.
[0061] Step 1: Preparation of SiO2@CeO2 microspheres: SiO2@CeO2 was prepared by homogeneous in situ precipitation method.
[0062] Silica microspheres (0.2 g) were ultrasonically dispersed in a mixed solution of water (50 mL) and ethanol (50 mL); Ce(NO3)3·6H2O (0.3 g) and hexamethylenetetramine (HMT) (0.2 g) were added in sequence; the temperature of the mixture was then raised to 70°C and kept at reflux for 4 h, and then cooled to room temperature. The product was purified by centrifugation (8000 rpm and 5 min), washed three times with water and dried at 60°C to obtain CeO2@SiO2 microspheres.
[0063] Step 2, preparation of SiO2@CeO2 / poly(VTMS) double-layer microspheres: SiO2@CeO2 / poly(VTMS) double-layer microspheres were prepared by hydrothermal method. The specific steps are as follows:
[0064] The SiO2@CeO2 microspheres (1.0 g) prepared in step 1 were ultrasonically dispersed in deionized water (70 mL) for 1 h. Urea (2.1 g) and sodium tartrate dihydrate (Na2C4H4O6·2H2O) (0.4 g) were added in sequence, and the suspension was mechanically stirred for 0.5 h; then VTMS (2 mL) was added, and the pH value of the solution was adjusted to 3-4 with 1 M HCl solution; after stirring for 1 h, the mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, sealed and maintained at 180 °C for 3 h. After cooling, the reaction mixture was centrifuged at 8500 rpm for 5 min, the product was collected, and washed three times with deionized water. The final product was obtained after drying at 80 °C overnight.
[0065] The CsPbBr3@SrHAp nanorods have a structure as shown in the attached Figure 1 As shown, it is prepared by the following steps:
[0066] Step 1, preparation of mesoporous SrHAp nanorods: based on a Ca / P and (Ca + Sr) / P molar ratio of 1.67, the nanorods were prepared by a hydrothermal method, wherein the Sr 2 + / (Ca 2 + + Sr 2+) molar ratio is 0.15;
[0067] First, 6 mmol Na2HPO4·12 H2O was dissolved in 50 mL of deionized water to form a solution (labeled as solution-1), and 1 mol / L NaOH solution was added to adjust the pH value of solution-1 to 11.5. Then, an aqueous solution (labeled as solution-2) containing 10 mmol (Ca(NO3)2·4H2O) and Sr(NO3)2 was prepared by dissolving them in 30 mL of deionized water. 2 + + Sr 2+ ), and slowly added to Solution-1 under magnetic stirring. Then, the obtained white milky suspension was transferred to a polytetrafluoroethylene-lined stainless steel autoclave (100 mL capacity), sealed, and kept at 200 °C for 8 h. Finally, under the condition of natural cooling of the autoclave, the precipitate was separated, washed with deionized water and ethanol in sequence, and the obtained powder was dried at 100 °C for 6 h.
[0068] Similarly, CaHAp nanorods not doped with strontium were set as a control group according to the above steps.
[0069] Step 2, preparation of CsPbBr3@SrHAp:
[0070] (1) Preparation of CsPbBr3 PQDs solution: Take a certain amount of CsPbBr3 PQDs and disperse them in a n-hexane solution to form a CsPbBr3 PQDs solution, in which the concentrations of CsPbBr3 PQDs are 5%, 10%, 15%, 20%, 25%, and 30% respectively;
[0071] (2) Preparation of CsPbBr3@SrHAp: The SrHAp sample obtained above was added to a n-hexane solution and stirred, and then CsPbBr3PQDs were injected into the n-hexane solution. The amount of SrHAp sample and n-hexane was m / s based on the total amount of n-hexane. SrHAp / V 正己烷 =1g / 100mL. Stir for 60-70min to fully mix SrHAp and CsPbBr3 PQDs. The complex was separated by centrifugation at 4000rpm and washed twice with n-hexane. Finally, the CsPbBr3@SrHAp nanocomposites were obtained by drying in a vacuum oven for 1h, which were denoted as CsPbBr3@SrHAp-5%, CsPbBr3@SrHAp-10%, CsPbBr3@SrHAp-15%, CsPbBr3@SrHAp-20%, CsPbBr3@SrHAp-25% and CsPbBr3@SrHAp-30%.
[0072] Furthermore, according to the above steps, CsPbBr3@SrHAp-15% and CsPbBr3@SrHAp-20% of CsPbBr3 quantum dot materials loaded with CaHAp nanorods without strontium were set as control groups.
[0073] Furthermore, according to the above steps, CsPbBr3@SiO2-15% and CsPbBr3@SiO2-20% of mesoporous silica particles loaded with CsPbBr3 quantum dot materials were set as control groups.
[0074] The mesoporous silica particles have a particle size of 100-150 nm, a purity of ≥ 99.9wt%, and a pore size of ~10 nm.
[0075] Example 1
[0076] The present invention provides a quantum dot coated reflective film, as shown in the attached Figure 3 As shown, it includes a substrate and a quantum dot glue layer formed by coating and curing a quantum dot glue composition on one side of the substrate. The quantum dot glue composition includes resin glue, optical particles, and additives; the optical particles include quantum dot particles and light diffusion particles; the quantum dot particles are CsPbBr3@SrHAp-5% nanorods; and the light diffusion particles are SiO2@CeO2 / poly(VTMS) microspheres.
[0077] A method for preparing a quantum dot coated reflective film is as follows:
[0078] Step 1: Preparation of quantum dot glue composition coating liquid according to the following formula:
[0079] 25 parts of tri(propylene glycol) diacrylate
[0080] Polyurethane acrylate 75 parts
[0081] Photoinitiator 184 2 parts
[0082] 8 parts of quantum dot particles
[0083] 2 pieces of light diffusion particles
[0084] Place the raw materials in a sealed container in the dark and stir them magnetically at room temperature at a speed of 50 to 200 rpm for 5 to 30 min to obtain a glue composition coating liquid after stirring evenly;
[0085] Step 2: Coat the quantum dot glue composition coating liquid on one side of a PET reflective base film, the thickness of the PET reflective base film is 150 μm, then place the film in a 100 W UV lamp (365 nm) for 10 minutes, and finally, bake it in an oven at 60 ° C for 24 hours to obtain a quantum dot coated reflective film, the thickness of the quantum dot glue layer is 8 μm.
[0086] Example 2
[0087] The quantum dot particles were adjusted to CsPbBr3@SrHAp-10%, and the remaining steps were consistent with Example 1.
[0088] Example 3
[0089] The quantum dot particles were adjusted to CsPbBr3@SrHAp-15%, and the remaining steps were consistent with Example 1.
[0090] Example 4
[0091] The quantum dot particles were adjusted to CsPbBr3@SrHAp-20%, and the remaining steps were consistent with Example 1.
[0092] Example 5
[0093] The quantum dot particles were adjusted to CsPbBr3@SrHAp-25%, and the remaining steps were consistent with Example 1.
[0094] Example 6
[0095] The quantum dot particles were adjusted to CsPbBr3@SrHAp-30%, and the remaining steps were consistent with Example 1.
[0096] Example 7
[0097] The quantum dot particles in the quantum dot adhesive layer composition were adjusted to 4 parts, and the remaining steps were consistent with Example 4.
[0098] Example 8
[0099] The quantum dot particles in the quantum dot adhesive layer composition were adjusted to 12 parts, and the remaining steps were consistent with Example 4.
[0100] Example 9
[0101] The amount of light diffusion dot particles in the quantum dot adhesive layer composition was adjusted to 1 part, and the remaining steps were consistent with Example 4.
[0102] Example 9
[0103] The light diffusion dot particles in the quantum dot glue layer composition were adjusted to 3 parts, and the remaining steps were consistent with Example 4.
[0104] Comparative Example 1
[0105] The quantum dot particles were adjusted to CsPbBr3@CaHAp-15%, and the remaining steps were consistent with Example 3.
[0106] Comparative Example 2
[0107] The quantum dot particles were adjusted to CsPbBr3@CaHAp-20%, and the remaining steps were consistent with Example 4.
[0108] Comparative Example 3
[0109] The quantum dot particles are adjusted to CsPbBr3@SiO2-15%, and the remaining steps are consistent with Example 3. The reflective film structure is as shown in the attached figure. Figure 4 shown.
[0110] Comparative Example 4
[0111] The quantum dot particles are adjusted to CsPbBr3@SiO2-20%, and the remaining steps are consistent with Example 4. The reflective film structure is as shown in the attached figure. Figure 4 shown.
[0112] Comparative Example 5
[0113] The quantum dot particles were adjusted to CsPbBr3, and the remaining steps were consistent with Example 4.
[0114] Comparative Example 6
[0115] The quantum dot particles were adjusted to SrHAp, and the remaining steps were consistent with Example 4.
[0116] Comparative Example 7
[0117] The light diffusion dot particles in the quantum dot glue layer composition were adjusted to 0 parts, and the remaining steps were consistent with Example 4.
[0118] Comparative Example 8
[0119] The quantum dot particles in the quantum dot adhesive layer composition were adjusted to 0 parts, and the remaining steps were consistent with Example 4.
[0120] Comparative Example 9
[0121] The quantum dot particles and light diffusion particles in the quantum dot adhesive layer composition were adjusted to 0 parts, and the remaining steps were consistent with Example 4.
[0122] Table 1 Summary of components of the optical particles in the subbing layer of Examples 1 to 10 and Comparative Examples 1 to 9
[0123]
[0124] The performance of the quantum dot-coated reflective film prepared by the present invention was evaluated:
[0125] (1) Brightness, brightness uniformity, and color coordinates test:
[0126] Refer to GB / T 43979-2024, use BM-7A brightness colorimeter to test the brightness, brightness uniformity and color coordinates of the sample; the higher the brightness uniformity, the more uniform the light output;
[0127] In addition, the film samples were aged for 1000 hours at 60°C and 90% RH and their brightness and color coordinates were tested again. The low drift of the brightness and color coordinates of the film after aging indicated that the film had good stability. The brightness attenuation was ≤10%, and the changes of the x-coordinate and y-coordinate were ≤0.01, which met the requirements.
[0128] (2) Mechanical properties test: Take 15 cm long and 15 mm wide membrane specimens, 3 in each MD / TD direction, and use a universal material testing machine to test the tensile strength under the conditions of a gauge length of 100 cm and a speed of 100 mm / min, and take the average value.
[0129] The test results are shown in Table 2.
[0130] Table 2 Test results of reflective films of Examples 1 to 10 and Comparative Examples 1 to 9
[0131]
[0132] It can be seen from the data in the above table that Examples 1 to 6 investigate the performance of the reflective film coated with the CsPbBr3@SrHAp quantum dot glue layer based on different concentrations of CsPbBr3 quantum dot particles. It can be found that the brightness of the films of Examples 3, 4, 5 and 6 is relatively higher, and the brightness uniformity is better. After aging, the brightness attenuation of the films is relatively low, and the x drift and y drift values are relatively smaller, indicating that the CsPbBr3@SrHAp particles loaded with CsPbBr3 quantum dot particles in this concentration range have better stability in the glue layer, and the quantum dot reflective film based thereon has better performance.
[0133] Example 4, Example 7, Example 8 and Comparative Example 8 investigated the performance of reflective films coated with CsPbBr3@CaHAp-20% particle glue layers based on 20% concentration CsPbBr3 quantum dot particles with different addition amounts. It can be found that the film material of Example 4 is much better in terms of brightness, brightness uniformity and stability. Among them, the brightness of the film material of Example 7 is low, and the comprehensive performance of the film material of Example 8 is not much different from that of Example 4. However, its tensile strength is slightly worse, indicating that excessive particle addition will affect the mechanical strength of the film material. This may be due to the combination of an appropriate amount of multi-morphology particles to form a multi-morphology particle glue layer with a network structure, which can make the polymer particles more evenly distributed, so that the particles produce a stress concentration effect in the organic system and further improve the mechanical strength of the reflective film. If too many particles are added, the bonding strength between the rigid particles and the glue layer is not high enough, which leads to interfacial fracture during stretching, thereby reducing the tensile strength.
[0134] Example 4, Example 9, Example 10 and Comparative Example 7 investigated the performance of the reflective film coated with SiO2@CeO2 / poly (VTMS) diffusion particle glue layer based on different added amounts, and found that the brightness uniformity of Comparative Example 7 was significantly worse than that of Example 4, Example 9 and Example 10, and the brightness and tensile strength of Comparative Example 7 were low, indicating that the synergistic effect of SiO2@CeO2 / poly (VTMS) diffusion particles and CsPbBr3@SrHAp-20% particles with different morphologies can improve the brightness and brightness uniformity of the film, and the appropriate dosage ratio can also help improve the mechanical properties of the film.
[0135] Comparative Examples 1 and 2 are quantum dot coated reflective films based on CaHAp loaded with 15% and 20% CsPbBr3, while Comparative Examples 3 and 4 are quantum dot glue layer reflective films based on mesoporous silica loaded with 15% and 20% CsPbBr3. By comparing Example 3 and Example 4 respectively, it can be found that the brightness of the reflective film based on mesoporous silica loaded with CsPbBr3 (Comparative Examples 3 and 4) is lower, and the brightness of the reflective film based on CaHAp loaded with CsPbBr3 quantum dots (Comparative Examples 1 and 2) is relatively low, and the stability of the glue layer reflective film based on mesoporous silica loading is worse than that based on CaHAp loading or SrHAp loading, the brightness attenuation of the film material after aging is higher, and the x drift and y drift values are relatively larger. This shows that the thermal stability of CsPbBr3 PQDs in the nanocomposite is significantly improved after being compounded with the SrHAp matrix, and the quantum dot film based on SrHAp loading has a higher brightness. This is because the mesoporous SrHAp nanorods with abundant surface hydroxyl groups and a larger aspect ratio can adsorb more CsPbBr3 particles than silica. In addition, SrHAp itself can emit very strong blue light, and its compound with CsPbBr3 PQDs that emit green light obtains a composite particle material. Due to the energy transfer between the two, the green light emission of CsPbBr3 PQDs is significantly enhanced.
[0136] Comparative Example 5 is an unloaded CsPbBr3 quantum dot reflective film, Comparative Example 6 is a SrHAp reflective film without added quantum dots, Comparative Example 8 is a reflective film with only SiO2@CeO2 / poly(VTMS) added, and Comparative Example 9 is a reflective film without added optical particles. By comparison, it can be found that the brightness of the CsPbBr3 quantum dot reflective film (Comparative Example 5) is significantly higher than that of Comparative Examples 8 and 9, and the brightness of the SrHAp reflective film (Comparative Example 6) is also higher than that of Comparative Examples 8 and 9. This may be due to the photoluminescence performance of SrHAp, and the brightness of the CsPbBr3 quantum dot reflective film (Comparative Example 5) is close to that of Example 5, further illustrating that the composite of SrHAp and CsPbBr3 PQDs can significantly enhance the luminescence performance of PQDs.
[0137] In summary, the present invention provides a quantum dot-coated reflective film and a preparation method thereof, wherein the CsPbBr3 quantum dots in the glue composition are loaded with SrHAp to improve their stability and at the same time improve the luminescence performance of PQDs; SiO2@CeO2 / poly(VTMS) diffusion particles improve the light emission uniformity of the film material; the synergistic effect of multi-morphology particles to form a multi-morphology particle glue layer with a network structure can make the polymer particles more evenly distributed, and further improve the mechanical strength of the reflective film and improve the scratch resistance of the film.
Claims
1. A quantum dot coated reflective film, comprising a reflective film substrate and a quantum dot glue layer formed by coating and curing a quantum dot glue composition disposed on one or more surfaces of the reflective film substrate, characterized in that: The quantum dot glue composition comprises resin glue, optical particles and additives; The optical particles are light diffusion particles and quantum dot particles; The resin glue is a mixture of tri(propylene glycol) diacrylate and polyurethane acrylate, and the usage ratio of tri(propylene glycol) diacrylate to polyurethane acrylate is 1:2.9-3.8 in parts by mass; The light diffusion particles are silica nanoparticle microspheres coated with a double layer of cerium dioxide and vinyltrimethoxysilane, denoted as SiO2@CeO2 / poly(VTMS) microspheres; The SiO2@CeO2 / poly(VTMS) microspheres are prepared in two steps. First, CeO2 is coated on the surface of SiO2 to obtain SiO2@CeO2 microspheres by a homogeneous in-situ precipitation method, and then poly(VTMS) is coated on the surface of SiO2@CeO2 microspheres by a hydrothermal method to obtain SiO2@CeO2 / poly(VTMS) double-layer microspheres. The quantum dot particles are mesoporous SrHAp nanorods loaded with CsPbBr3 quantum dots, denoted as CsPbBr3@SrHAp nanorods; The mesoporous SrHAp nanorods are strontium-doped hydroxyapatite, wherein the molar ratio of the total amount of Ca and Sr to P is 1.67; 2+ / (Ca 2+ +Sr 2+ ) molar ratio is 0.10 or 0.15; The optical particles account for 5-15% of the weight of the resin glue; the quantum dot particles account for 60-90% of the weight of the optical particles.
2. A quantum dot coated reflective film according to claim 1, characterized in that: The auxiliary agent includes a photoinitiator, and the photoinitiator includes a photoinitiator 184; the photoinitiator accounts for 1 to 3% of the weight of the resin glue.
3. A quantum dot coated reflective film according to claim 2, characterized in that: The SiO2@CeO2 / poly(VTMS) microspheres are prepared by the following steps: Step 1, preparation of SiO2@CeO2 microspheres: SiO2@CeO2 was prepared by homogeneous in-situ precipitation method; The specific preparation steps are as follows: ultrasonically dispersing silica microspheres in a mixed solution of water and ethanol to prepare a 0.2wt% dispersion; adding Ce(NO3)3·6H2O and HMT in sequence, then raising the temperature of the mixture to 70°C and keeping it under reflux for 4h, and then cooling it to room temperature; then purifying the product by centrifugation, washing with water and drying at 60°C to obtain CeO2@SiO2 microspheres; Step 2, preparation of SiO2@CeO2 / poly(VTMS) double-layer microspheres: preparing SiO2@CeO2 / poly(VTMS) double-layer microspheres by hydrothermal method; The specific preparation steps are as follows: ultrasonically disperse the SiO2@CeO2 microspheres prepared in step 1 in deionized water for 1 hour; add urea and sodium tartrate dihydrate in sequence; mechanically stir the suspension for 0.5 hour; then add vinyltrimethoxysilane, adjust the pH value of the solution to 3-4 with 1M HCl solution and stir for 1 hour, transfer the mixed solution to a polytetrafluoroethylene-lined stainless steel autoclave, seal it and maintain it at 180°C for 3 hours; after cooling, centrifuge the reaction mixture, wash it with deionized water and dry it at 80°C overnight to obtain the final product.
4. A quantum dot coated reflective film according to claim 3, characterized in that: In the preparation step of the SiO2@CeO2 microspheres, the volume ratio of water to ethanol is 1:1; the mass ratio of Ce(NO3)3·6H2O to HMT is 3:
2.
5. The quantum dot coated reflective film according to claim 3, characterized in that: In the preparation step of the SiO2@CeO2 / poly(VTMS) double-layer microspheres, the amount of SiO2@CeO2 microspheres and deionized water is m SiO2@CeO2 / V 去离子水 =1g / 70mL; the amount of SiO2@CeO2 microspheres, Na2C4H4O6·2H2O and urea is 1:21:4 by mass; the amount of SiO2@CeO2 microspheres and VTMS is m SiO2@CeO2 / V VTMS =1g / 2mL.
6. A quantum dot coated reflective film according to claim 5, characterized in that: The length of the mesoporous SrHAp nanorod is 120-150 nm, the diameter is 20 nm, and the diameter of the mesoporous structure is 5-15 nm; the particle size of the CsPbBr3 PQDs is 1-10 nm.
7. A quantum dot coated reflective film according to claim 6, characterized in that: The CsPbBr3@SrHAp nanorods are obtained by the following steps: Step 1, preparation of CsPbBr3 PQDs solution: dispersing CsPbBr3 PQDs into n-hexane solution to form a CsPbBr3 PQDs solution, wherein the concentration of PQDs is 5 to 30 wt%; Step 2, preparation of CsPbBr3@SrHAp: add the SrHAp sample to the n-hexane solution and stir; then inject the CsPbBr3 PQDs solution obtained in step 1 into the above n-hexane solution and stir for 60 to 70 minutes to fully mix the SrHAp and CsPbBr3 PQDs, separate the complex by centrifugation, wash with n-hexane, and dry in a vacuum oven for 1 hour to obtain the CsPbBr3@SrHAp nanocomposite.
8. The quantum dot coated reflective film according to claim 7, characterized in that: In the step 2, based on the total amount of n-hexane, the amount of SrHAp sample and n-hexane is m SrHAp / V 正己烷 =1g / 100mL.
9. A method for preparing a quantum dot-coated reflective film according to any one of claims 1 to 8, characterized in that: The steps include: Step 1, preparation of quantum dot glue composition coating liquid, placing the raw materials in a closed container according to the formula in the dark and magnetically stirring at room temperature, the stirring speed is 50-200 rpm, the stirring time is 5-30 min, and the glue composition coating liquid is obtained after stirring evenly; Step 2: Coat the quantum dot glue composition coating liquid on one or both sides of the PET reflective base film, then place the film in a 100W UV lamp for 10 minutes on each side, and finally bake it in an oven at 60°C for 24 hours to obtain a coated reflective film based on the quantum dot glue layer.