Rare earth composite photo-thermal stabilizer as well as preparation method, application and composition thereof
By combining rare earth-benzophenone complexes with organic zinc, rare earth composite photothermal stabilizers are prepared, and antioxidants and other ingredients are added to chlorinated polyvinyl chloride to solve the problem of chlorinated polyvinyl chloride under the action of light and heat. stability issues, significantly improving its thermal stability and light stability.
Patent Information
- Application Number
- CN202411029330.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-01
AI Technical Summary
The effectiveness of existing rare earth composite stabilizers in improving the photothermal stability of chlorinated polyvinyl chloride still needs to be improved, and CPVC is easily degraded and removes HCl under the action of light and heat, resulting in poor stability.
Rare earth-benzophenone complexes are combined with organic zinc, and rare earth composite photothermal stabilizers are prepared by reacting water-soluble rare earth inorganic salts with specific compounds, and antioxidants, auxiliary stabilizers, and lubrication are added to chlorinated polyvinyl chloride. agents and excipients to improve thermal stability and light stability.
Significantly improves the thermal stability and light stability of chlorinated polyvinyl chloride, extends its tensile strength and stability time after UV aging, and enhances its durability at high temperatures.
Smart Images

Figure BDA0004969486800000021 
Figure BDA0004969486800000041 
Figure FDA0004969486790000011
Abstract
Description
Technical Field
[0001] The invention relates to a rare earth composite light and heat stabilizer and a preparation method, application and composition thereof. Background Art
[0002] Chlorinated polyvinyl chloride (CPVC) has better aging resistance, corrosion resistance and high temperature resistance than PVC. This good comprehensive performance makes CPVC resin widely used in pipes, plates, insulation and flame retardant materials, artificial fibers, blending and modification, etc. CPVC has poor stability during processing and use, and is very easy to release HCl under the action of light and heat. This is due to the presence of various structural defects in the CPVC molecular chain. Since the chlorine content of CPVC is higher than that of PVC, the stability of CPVC is worse and it needs to be used with a stabilizer.
[0003] CN110330686A discloses a rare earth composite stabilizer, comprising a praseodymium-benzophenone complex and a stearate. The 2-position of the benzophenone compound is substituted by a hydroxyl group, and the 4-position is substituted by an alkyl group. The stearate is selected from a stearate of a metal of Group IIA, a stearate of a metal of Group IIIA, or a stearate of a metal of Group IIIB. The rare earth composite stabilizer still needs to be improved in terms of improving the light and heat stability of chlorinated polyvinyl chloride.
[0004] CN11344328A discloses a PVC primary stabilizer, which is a rare earth complex with a benzophenone structure. The compound of the benzophenone structure is one or more combinations of 2-(4-methylbenzoyl)benzoic acid, 4-hydroxybenzophenone, 2-benzoylbenzoic acid, 2-hydroxybenzophenone, and 4-propyleneoxy-2-hydroxybenzophenone. The effect of this stabilizer on improving the light and heat stability of chlorinated polyvinyl chloride still needs to be improved. Summary of the invention
[0005] In view of this, one object of the present invention is to provide a rare earth composite light and heat stabilizer, which can effectively improve the thermal stability and light stability of chlorinated polyvinyl chloride. Another object of the present invention is to provide a method for preparing a rare earth composite light and heat stabilizer. Another object of the present invention is to provide a use of a rare earth composite light and heat stabilizer. Another object of the present invention is to provide a chlorinated polyvinyl chloride composition, which has excellent thermal stability and light stability.
[0006] The above purpose is achieved through the following technical solutions.
[0007] In one aspect, the present invention provides a rare earth composite light and heat stabilizer, comprising a rare earth-benzophenone complex and organic zinc; the rare earth-benzophenone complex is obtained by reacting a water-soluble rare earth inorganic salt with a compound represented by formula (I):
[0008]
[0009] Among them, R 1 is an alkoxy group, R 2 is a sulfonic acid group;
[0010] The organic zinc is selected from one or more of zinc stearate, zinc salicylate, zinc laurate and zinc ricinoleate.
[0011] According to the rare earth composite light and heat stabilizer of the present invention, preferably, the R 1 It is an alkoxy group having 1 to 6 carbon atoms.
[0012] According to the rare earth composite light and heat stabilizer of the present invention, preferably, the rare earth-benzophenone complex is 1.2 parts by weight, and the organic zinc is 2 to 8 parts by weight.
[0013] According to the rare earth composite light and heat stabilizer of the present invention, preferably, the composite light stabilizer further comprises an antioxidant, an auxiliary stabilizer, a lubricant and auxiliary materials;
[0014] The antioxidant is selected from one or more of antioxidant 168, antioxidant 215, antioxidant 1010, and antioxidant 1076;
[0015] The auxiliary stabilizer is selected from one or more of dipentaerythritol, stearyl benzoyl methane, and epoxidized soybean oil;
[0016] The lubricant is selected from one or more of polyethylene wax, Fischer-Tropsch wax, oxidized polyethylene wax, and stearic acid;
[0017] The auxiliary material is selected from one or more of light calcium carbonate, kaolin, talc and zeolite.
[0018] According to the rare earth composite light and heat stabilizer of the present invention, preferably, the rare earth composite light and heat stabilizer also includes 0.1 to 1 weight parts of antioxidant 1010, 1 to 3.5 weight parts of dipentaerythritol, 0.1 to 1 weight parts of stearyl benzoyl methane, 0.3 to 1.5 weight parts of epoxidized soybean oil, 0.5 to 3 weight parts of polyethylene wax, 0.5 to 3 weight parts of oxidized polyethylene wax 316, 0.1 to 1 weight parts of oxidized polyethylene wax 629, 2 to 10 weight parts of kaolin and 1 to 4 weight parts of zeolite.
[0019] On the other hand, the present invention provides a method for preparing the rare earth composite light and heat stabilizer, comprising the following steps:
[0020] (1) mixing an aqueous solution of a water-soluble rare earth inorganic salt with an ethanol solution of a compound represented by formula (I), adjusting the pH value to 6 to 7 with a 0.1 to 1.0 mol / L ammonia solution, and then reacting at 20 to 35° C. for 1 to 10 hours to obtain a rare earth-benzophenone complex;
[0021] (2) Mixing raw materials including rare earth-benzophenone complex and organic zinc uniformly to obtain a rare earth composite light and heat stabilizer.
[0022] According to the preparation method of the present invention, preferably, the molar ratio of the rare earth element in the water-soluble rare earth inorganic salt to the compound represented by formula (I) is 1:1-5; the concentration of the water-soluble inorganic salt in the aqueous solution is 0.1-0.5 mol / L, and the concentration of the compound represented by formula (I) in the ethanol solution is 0.3-1.5 mol / L.
[0023] In yet another aspect, the present invention provides use of the rare earth composite light and heat stabilizer in improving the thermal stability and / or light stability of chlorinated polyvinyl chloride.
[0024] In another aspect, the present invention provides a chlorinated polyvinyl chloride composition, comprising 100 parts by weight of chlorinated polyvinyl chloride and 5 to 15 parts by weight of the above-mentioned rare earth composite light and heat stabilizer.
[0025] The chlorinated polyvinyl chloride composition according to the present invention preferably further comprises 10 to 20 parts by weight of light calcium carbonate, 2 to 15 parts by weight of chlorinated polyethylene and 1 to 5 parts by weight of titanium dioxide.
[0026] The rare earth composite light and heat stabilizer of the present invention can simultaneously improve the thermal stability and light stability of chlorinated polyvinyl chloride. The components in the rare earth composite light and heat stabilizer of the present invention cooperate with each other to achieve better thermal stability and light stability effects. The chlorinated polyvinyl chloride composition to which the rare earth composite light and heat stabilizer of the present invention is added has higher tensile strength after ultraviolet aging. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0028] <Rare earth composite light and heat stabilizer>
[0029] The rare earth composite light and heat stabilizer of the present invention comprises a rare earth-benzophenone complex and organic zinc. The rare earth composite light and heat stabilizer of the present invention may also comprise an antioxidant, an auxiliary stabilizer, a lubricant and auxiliary materials, etc. In certain embodiments, the rare earth composite light and heat stabilizer of the present invention consists only of the above ingredients.
[0030] The rare earth-benzophenone complex of the present invention is obtained by reacting a water-soluble rare earth inorganic salt with a compound represented by formula (I):
[0031]
[0032] Among them, R 1 is an alkoxy group, R 2 It is a sulfonic acid group.
[0033] Preferably, R 1 is an alkoxy group containing 1 to 6 carbon atoms; more preferably, R 1 It is an alkoxy group containing 1 to 3 carbon atoms.
[0034] Examples of alkoxy groups include, but are not limited to, methoxy, ethoxy, propoxy, butoxy, methylpropyloxy, pentyloxy, methylbutyloxy, ethylpropyloxy, hexyloxy, methylpentyloxy, dimethylbutyloxy, ethylbutyloxy.
[0035] According to one embodiment of the present invention, the compound represented by formula (I) is 2-hydroxy-4-methoxy-5-sulfonic acid-benzophenone.
[0036] In the present invention, the rare earth element in the water-soluble rare earth inorganic salt is preferably Y. The present invention finds that the complex formed by Y and the above-mentioned organic ligand can better improve the thermal stability and light stability of chlorinated polyvinyl chloride. The water-soluble rare earth inorganic salt can be rare earth chloride or rare earth nitrate. According to one embodiment of the present invention, the water-soluble rare earth inorganic salt is yttrium nitrate.
[0037] According to one embodiment of the present invention, the rare earth-benzophenone complex is obtained by reacting a water-soluble inorganic yttrium salt with 2-hydroxy-4-methoxy-5-sulfonic acid-benzophenone, which can better improve the light stability and thermal stability of chlorinated polyvinyl chloride.
[0038] The organic zinc is selected from one or more of zinc stearate, zinc salicylate, zinc laurate and zinc ricinoleate. Preferably, the organic zinc is zinc ricinoleate. In this way, it can be combined with the rare earth-benzophenone complex of the present invention to achieve the effect of better improving the light stability and thermal stability of chlorinated polyvinyl chloride.
[0039] Based on 1.2 parts by weight of the rare earth-benzophenone complex, the amount of organic zinc used can be 2 to 8 parts by weight, preferably 3 to 7 parts by weight, and more preferably 5 to 6 parts by weight.
[0040] The antioxidant of the present invention can be selected from one or more of antioxidant 168, antioxidant 215, antioxidant 1010, and antioxidant 1076. Preferably, the antioxidant is antioxidant 1010.
[0041] Based on 1.2 parts by weight of the rare earth-benzophenone complex, the amount of the antioxidant used can be 0.1 to 1; preferably 0.3 to 0.8 parts by weight; more preferably 0.6 to 0.7 parts by weight.
[0042] The auxiliary stabilizer of the present invention can be selected from one or more of dipentaerythritol, stearylbenzoylmethane, and epoxidized soybean oil. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of the auxiliary stabilizer can be 1 to 7 parts by weight; preferably 2 to 5 parts by weight; more preferably 3 to 4 parts by weight. Preferably, the auxiliary stabilizer is a combination of dipentaerythritol, stearylbenzoylmethane and epoxidized soybean oil. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of dipentaerythritol is 1 to 3.5 parts by weight; preferably 2 to 2.5 parts by weight. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of stearylbenzoylmethane is 0.1 to 1 part by weight; preferably 0.4 to 0.6 parts by weight. Based on 1.2 parts by weight of the rare earth-benzophenone complex, the amount of the epoxy soybean oil used is 0.3 to 1.5 parts by weight, preferably 0.8 to 1 part by weight.
[0043] The lubricant of the present invention can be selected from one or more of polyethylene (PE) wax, Fischer-Tropsch wax, oxidized polyethylene (OPE) wax, and stearic acid. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of lubricant can be 1 to 7 parts by weight; preferably 2 to 5 parts by weight; more preferably 3 to 4 parts by weight. Preferably, the lubricant is a combination of polyethylene wax, oxidized polyethylene wax 316, and oxidized polyethylene wax 629. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of polyethylene wax can be 0.5 to 3 parts by weight; preferably 1.5 to 2 parts by weight. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of oxidized polyethylene wax 316 can be 0.5 to 3 parts by weight; preferably 1.2 to 1.5 parts by weight. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of oxidized polyethylene wax 629 can be 0.1 to 1 parts by weight; more preferably 0.6 to 0.8 parts by weight.
[0044] The auxiliary material of the present invention can be selected from one or more of light calcium carbonate, kaolin, talc, and zeolite. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of auxiliary material can be 5 to 20 parts by weight; preferably 7 to 15 parts by weight; more preferably 8 to 10 parts by weight. Preferably, the auxiliary material is a combination of kaolin and zeolite. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of kaolin can be 2 to 10 parts by weight; preferably 6 to 8 parts by weight. Based on 1.2 parts by weight of rare earth-benzophenone complexes, the amount of zeolite can be 1 to 4 parts by weight; preferably 2 to 3 parts by weight.
[0045] The rare earth composite light and heat stabilizer composed of the above mentioned components has good dispersibility in chlorinated polyvinyl chloride, and the above mentioned components cooperate with each other to further improve the heat stability and light stabilizer of chlorinated polyvinyl chloride.
[0046] <Preparation method of rare earth composite light and heat stabilizer>
[0047] The method for preparing the rare earth composite light and heat stabilizer of the present invention comprises the following steps: (1) a preparation step of a rare earth-benzophenone complex; and (2) a formation step of a stabilizer.
[0048] In step (1), an aqueous solution of a water-soluble rare earth inorganic salt is mixed with an ethanol solution of a compound represented by formula (I), the pH value is adjusted with an aqueous ammonia solution, and then reacted to obtain a rare earth-benzophenone complex.
[0049] The molar ratio of the rare earth element in the water-soluble rare earth inorganic salt to the compound represented by formula (I) can be 1:(1-5); preferably 1:(1-4); more preferably 1:(1-3).
[0050] In step (1), the concentration of the water-soluble inorganic salt in the aqueous solution may be 0.1 to 0.5 mol / L, and the concentration of the compound represented by formula (I) in the ethanol solution is 0.3 to 1.5 mol / L. Preferably, the concentration of the water-soluble inorganic salt in the aqueous solution is 0.15 to 0.35 mol / L, and the concentration of the compound represented by formula (I) in the ethanol solution is 0.4 to 1 mol / L. More preferably, the concentration of the water-soluble inorganic salt in the aqueous solution is 0.2 to 0.25 mol / L, and the concentration of the compound represented by formula (I) in the ethanol solution is 0.5 to 0.6 mol / L.
[0051] In step (1), the concentration of ammonia water can be 0.1-1.0 mol / L; preferably, the concentration of ammonia water is 0.2-0.8 mol / L; more preferably, the concentration of ammonia water is 0.4-0.6 mol / L. The pH value is adjusted to 6-7 by ammonia water; preferably, the pH value is adjusted to 6.2-6.8 by ammonia water; more preferably, the pH value is adjusted to 6.4-6.6 by ammonia water. The reaction conditions are 20-35°C for 1-10 hours; preferably, the reaction conditions are 25-30°C for 2-8 hours; more preferably, the reaction conditions are 25-28°C for 2-3 hours. The reaction can be carried out under stirring.
[0052] The selection of the water-soluble rare earth inorganic salt and the compound represented by formula (I) is specifically as described above and will not be repeated here.
[0053] In step (2), the raw materials including the rare earth-benzophenone complex and the organic zinc are uniformly mixed to obtain a rare earth composite stabilizer. The raw materials of the rare earth composite stabilizer of the present invention may also include antioxidants, auxiliary stabilizers, lubricants and auxiliary materials. The selection and dosage of the above raw materials are specifically as described above and will not be repeated here.
[0054] <Application and chlorinated polyvinyl chloride composition>
[0055] The use of the rare earth composite light and heat stabilizer of the present invention in chlorinated polyvinyl chloride can simultaneously improve the thermal stability and light stability. Therefore, the present invention also provides the use of the above-mentioned rare earth composite light and heat stabilizer in improving the thermal stability and / or light stability of chlorinated polyvinyl chloride. Preferably, the use of the above-mentioned rare earth composite light and heat stabilizer in simultaneously improving the thermal stability and light stability of chlorinated polyvinyl chloride.
[0056] The chlorinated polyvinyl chloride composition of the present invention comprises 100 parts by weight of chlorinated polyvinyl chloride and 1 to 15 parts by weight of a rare earth composite light and heat stabilizer. Preferably, the amount of the rare earth composite light and heat stabilizer is 4 to 12 parts by weight; more preferably, the amount of the rare earth composite light and heat stabilizer is 6 to 8 parts by weight.
[0057] The chlorinated polyvinyl chloride composition of the present invention may further include light calcium carbonate, chlorinated polyethylene and titanium dioxide. According to one embodiment of the present invention, the chlorinated polyvinyl chloride composition consists only of the above components.
[0058] The amount of light calcium carbonate used can be 10 to 20 parts by weight, preferably 12 to 18 parts by weight, and more preferably 15 to 16 parts by weight.
[0059] The amount of chlorinated polyethylene used may be 2 to 15 parts by weight, preferably 4 to 12 parts by weight, and more preferably 6 to 8 parts by weight.
[0060] The amount of titanium dioxide used can be 1 to 5 parts by weight, preferably 1.5 to 4 parts by weight, and more preferably 2 to 3 parts by weight.
[0061] Example 1
[0062] 0.01 mol yttrium nitrate (Y(NO 3 ) 3 ) is dissolved in 50 mL of water to form an aqueous solution of yttrium nitrate. 0.03 mol of 2-hydroxy-4-methoxy-5-sulfonic acid-benzophenone is dissolved in 50 mL of ethanol to form an ethanol solution of benzophenone compounds. The aqueous solution of yttrium nitrate and the above ethanol solution are mixed evenly to obtain a mixed solution. The mixed solution is adjusted to pH 6.5 with 0.5 mol / L of ammonia water, and then reacted for 2 hours at a temperature of 25°C and stirred to produce a precipitate. The precipitate is washed, filtered and dried in sequence to obtain a rare earth-benzophenone complex.
[0063] 1.2 parts by weight of rare earth-benzophenone complex, 5 parts by weight of zinc ricinoleate, 0.6 parts by weight of antioxidant 1010, 2 parts by weight of dipentaerythritol, 0.4 parts by weight of stearylbenzoylmethane, 0.8 parts by weight of epoxidized soybean oil, 1.5 parts by weight of polyethylene wax, 1.2 parts by weight of oxidized polyethylene wax 316, 0.6 parts by weight of oxidized polyethylene wax 629, 6 parts by weight of kaolin and 2 parts by weight of zeolite are uniformly mixed to obtain a rare earth composite light and heat stabilizer.
[0064] 100 parts by weight of CPVC (chlorinated polyvinyl chloride), 15 parts by weight of light calcium carbonate, 8 parts by weight of chlorinated polyethylene, 3 parts by weight of titanium dioxide and 8 parts by weight of rare earth composite light and heat stabilizer were mixed, placed on a double-roll plasticizer (roller temperature 180°C, roller distance 1mm) for plasticization for 5 minutes, and cut into square samples.
[0065] Comparative Example 1
[0066] 0.01 mol europium nitrate (Eu(NO 3 ) 3 ) is dissolved in 50mL of water to form an aqueous europium nitrate solution. 0.03mol of 2-hydroxy-4-ethoxy-benzophenone is dissolved in 50mL of ethanol to form an ethanol solution of a benzophenone compound. The europium nitrate aqueous solution and the above-mentioned ethanol solution are mixed evenly to obtain a mixed solution. The mixed solution is adjusted to pH 6.5 with 0.5mol / L of ammonia water, and then reacted for 2h at a temperature of 25°C and stirred to produce a precipitate. The precipitate is washed, filtered and dried in sequence to obtain a rare earth-benzophenone complex.
[0067] 1 part by weight of a rare earth-benzophenone complex, 5 parts by weight of zinc laurate, 0.5 parts by weight of antioxidant 215, 2.8 parts by weight of dipentaerythritol, 0.8 parts by weight of epoxidized soybean oil, 1.5 parts by weight of Fischer-Tropsch wax, 1.2 parts by weight of oxidized polyethylene wax 316, 0.6 parts by weight of oxidized polyethylene wax 629, and 6 parts by weight of talc are uniformly mixed to obtain a rare earth composite light and heat stabilizer.
[0068] 100 parts by weight of CPVC, 15 parts by weight of light calcium carbonate, 8 parts by weight of chlorinated polyethylene, 3 parts by weight of titanium dioxide and 8 parts by weight of rare earth composite light and heat stabilizer were mixed, placed on a double-roll plasticizer (roller temperature 180°C, roller distance 1mm) for plasticization for 5 minutes, and cut into square samples.
[0069] Experimental example
[0070] 1. Hot air exposure test
[0071] According to the hot air exposure test method for plastics (GB / T7141-92), the square samples were placed in an aging oven and subjected to an aging test at 180±1°C. The samples were taken out every 10 minutes to observe and record the changes in chromaticity. The experimental results are shown in Table 1.
[0072] Table 1. Oven aging results
[0073] Aging time (min) Example 1 Comparative Example 1 0 White White 10 White Light yellow 20 Light yellow Light yellow 30 yellow yellow 40 yellow Light Orange 50 brown brown 60 Dark Brown Dark Brown
[0074] It can be seen from Table 1 that the rare earth composite light and heat stabilizer of the present invention has a longer thermal stability time, which indicates that the rare earth composite light and heat stabilizer of the present invention has better thermal stability.
[0075] 2. Torque rheology experiment
[0076] A mixed sample containing CPVC was prepared according to the composition of the embodiment or the comparative example, and 70 grams of the sample was subjected to a torque rheological test on a Haake rheometer, with the torque rheological temperature set at 190° C. and the rotation speed set at 35 r / min. The experimental results are shown in Table 2.
[0077] Table 2. Torque rheological results
[0078] serial number Example 1 Comparative Example 1 Plasticizing time / min 1.48 2.04 Balance torque / Nm 17.43 18.25 Stabilization time / min 21.27 19.72
[0079] It can be seen from Table 2 that the rare earth composite light and heat stabilizer of the present invention has a longer stability time, which indicates that the rare earth composite light and heat stabilizer of the present invention has good long-term stability.
[0080] 3. UV aging test
[0081] The samples were cut into 4cm×3cm, 8 samples were cut from each sample, and placed in a QUV UV aging box for 168 hours of QUV UV aging experiment. The experimental temperature was 50°C, and a sample was taken from each sample every 24 hours. The changes in the sample chromaticity (Lab value) were observed and recorded by a colorimeter, and the ΔE value compared with the initial color chip was calculated. The experimental results are shown in Table 3.
[0082] Table 3. Chromaticity ΔE change results
[0083] Irradiation time (h) Example 1 Comparative Example 1 0 / / 24 2.31 2.66 48 2.65 2.93 72 2.98 3.29 96 3.68 4.01 120 4.29 4.60 144 4.87 5.18 168 5.11 5.63
[0084] According to the test method for tensile properties of plastics (GB / T1040-2006), the samples were cut into dumbbell shapes, and 6 specimens were cut from each sample and divided into two groups. One group was placed in a QUV UV aging box for a 168-hour QUV UV aging test. The changes in tensile strength and tensile elongation of each sample before and after aging were tested respectively. Each sample in each group was measured three times, and the average value was recorded. The experimental results are shown in Table 4.
[0085] Table 4. Test results of tensile strength and tensile elongation before and after aging
[0086] serial number Example 1 Comparative Example 2 Average tensile strength before aging / MPa 27.24 27.33 Average tensile strength after aging / MPa 30.12 27.49 Average tensile elongation before aging / % 15.22 17.65 Average tensile elongation after aging / % 14.33 15.27
[0087] As can be seen from Table 4, the tensile strength and tensile elongation of the CPVC composition of the present invention are comparable before and after aging, or even improved. This indicates that the rare earth composite light and heat stabilizer of the present invention has a better light stabilization effect.
[0088] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A rare earth composite light and heat stabilizer, characterized in that: The rare earth composite light and heat stabilizer comprises a rare earth-benzophenone complex and organic zinc; the rare earth-benzophenone complex is obtained by reacting a water-soluble rare earth inorganic salt with a compound represented by formula (I): Wherein, R1 is an alkoxy group, and R2 is a sulfonic acid group; The organic zinc is selected from one or more of zinc stearate, zinc salicylate, zinc laurate and zinc ricinoleate.
2. The rare earth composite light and heat stabilizer according to claim 1, characterized in that: The R1 is an alkoxy group containing 1 to 6 carbon atoms.
3. The rare earth composite light and heat stabilizer according to claim 1, characterized in that: The rare earth-benzophenone complex is 1.2 parts by weight, and the organic zinc is 2-8 parts by weight.
4. The rare earth composite light and heat stabilizer according to claim 1, characterized in that: The composite light stabilizer also includes an antioxidant, an auxiliary stabilizer, a lubricant and auxiliary materials; The antioxidant is selected from one or more of antioxidant 168, antioxidant 215, antioxidant 1010, and antioxidant 1076; The auxiliary stabilizer is selected from one or more of dipentaerythritol, stearyl benzoyl methane, and epoxidized soybean oil; The lubricant is selected from one or more of polyethylene wax, Fischer-Tropsch wax, oxidized polyethylene wax, and stearic acid; The auxiliary material is selected from one or more of light calcium carbonate, kaolin, talc and zeolite.
5. The rare earth composite light and heat stabilizer according to claim 1, characterized in that: The rare earth composite light and heat stabilizer also includes 0.1 to 1 weight parts of antioxidant 1010, 1 to 3.5 weight parts of dipentaerythritol, 0.1 to 1 weight parts of stearyl benzoyl methane, 0.3 to 1.5 weight parts of epoxidized soybean oil, 0.5 to 3 weight parts of polyethylene wax, 0.5 to 3 weight parts of oxidized polyethylene wax 316, 0.1 to 1 weight parts of oxidized polyethylene wax 629, 2 to 10 weight parts of kaolin and 1 to 4 weight parts of zeolite.
6. The method for preparing the rare earth composite light and heat stabilizer according to any one of claims 1 to 5, characterized in that: The steps include: (1) mixing an aqueous solution of a water-soluble rare earth inorganic salt with an ethanol solution of a compound represented by formula (I), adjusting the pH value to 6 to 7 with a 0.1 to 1.0 mol / L ammonia solution, and then reacting at 20 to 35° C. for 1 to 10 hours to obtain a rare earth-benzophenone complex; (2) Mixing raw materials including rare earth-benzophenone complex and organic zinc uniformly to obtain a rare earth composite light and heat stabilizer.
7. The preparation method according to claim 6, characterized in that: The molar ratio of the rare earth element in the water-soluble rare earth inorganic salt to the compound represented by formula (I) is 1:1-5; the concentration of the water-soluble inorganic salt in the aqueous solution is 0.1-0.5 mol / L, and the concentration of the compound represented by formula (I) in the ethanol solution is 0.3-1.5 mol / L.
8. Use of the rare earth composite light and heat stabilizer according to claim 1 in improving the thermal stability and / or light stability of chlorinated polyvinyl chloride.
9. A chlorinated polyvinyl chloride composition, characterized in that: The chlorinated polyvinyl chloride composition comprises 100 parts by weight of chlorinated polyvinyl chloride and 5 to 15 parts by weight of the rare earth composite light and heat stabilizer according to any one of claims 1 to 5.
10. The chlorinated polyvinyl chloride composition according to claim 9, characterized in that It also includes 10 to 20 parts by weight of light calcium carbonate, 2 to 15 parts by weight of chlorinated polyethylene and 1 to 5 parts by weight of titanium dioxide.
Citation Information
Patent Citations
Rare earth composite stabilizer, preparation method and application thereof
CN110330686A