High-mechanical-property graphene rubber containing modified porous starch as well as preparation method and application of high-mechanical-property graphene rubber
Through the synergistic effect of modified porous starch and graphene oxide, the problems of uneven dispersion of porous starch and weak interfacial interaction of graphene oxide are solved, significantly improving the mechanical properties and processing stability of rubber, and maintaining good performance in humid environments. performance.
Patent Information
- Application Number
- CN202411021157.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
AI Technical Summary
The uneven dispersion and hygroscopicity of porous starch in rubber lead to dimensional instability, and the interface interaction between graphene oxide and non-polar rubber matrix is weak, resulting in difficulty in dispersion and low reinforcement efficiency.
Using modified porous starch and modified graphene oxide, through esterification of dodecyl succinic anhydride and ball milling of polyvinylpyrrolidone, its compatibility and compatibility in natural rubber are improved, and through specific formulas and process steps Synthetic graphene rubber with high mechanical properties.
The mechanical properties and processing stability of rubber are significantly improved. The synergistic effect of modified porous starch and graphene oxide improves the tensile and tear strength of rubber and maintains good mechanical properties in humid environments.
Smart Images

Figure BDA0004967303210000071 
Figure BDA0004967303210000072 
Figure BDA0004967303210000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber manufacturing, and in particular to a high-mechanical-performance graphene rubber containing modified porous starch, and a preparation method and application thereof. Background Art
[0002] Porous starch is a new type of modified starch. It is formed by the action of enzymes with raw starch activity on raw starch at a temperature below the gelatinization temperature to form a porous honeycomb product. Porous starch can be used as a reinforcing filler for natural rubber or synthetic rubber. Its porous structure can increase the contact area inside the material, which may improve the mechanical properties of rubber composites, such as tensile strength and wear resistance. At the same time, compared with traditional inorganic fillers (such as carbon black, white carbon black, etc.), porous starch is easier to process and environmentally friendly. It can also improve the fluidity and processability of rubber mixtures, help reduce energy consumption and improve production efficiency. Its good oil absorption also helps to absorb and fix the oil components in the formula, reducing the greasy feeling during processing. Although porous starch has many potential advantages in rubber preparation, there are also some defects and challenges: the surface of porous starch is covered with small pores with a diameter of about 1μm. These small pores penetrate from the surface to the center, making the volume of the pores account for about 50% of the particle volume. But the abundant hydroxyl groups in the polymer structure of starch and its large particle size will not simply lead to the overall performance enhancement of starch / rubber composites as expected in theory. In reality, they will inevitably induce aggregation / low dispersion of starch particles, poor compatibility with the rubber matrix, further leading to uneven dispersion of fillers in rubber, forming agglomeration phenomena, affecting the uniformity of the material, and further limiting its strengthening function for rubber. In addition, porous starch has strong hygroscopicity, which may cause rubber products to absorb water and swell in humid environments, affecting dimensional stability and mechanical properties. This is an important issue for rubber products that require high dimensional stability.
[0003] Graphene oxide (GO) is one of the ideal reinforcing and functional fillers in rubber nanocomposites due to its ultra-high mechanical strength, large surface area, good barrier properties, high aspect ratio, water solubility and multifunctional surface properties. The introduction of graphene oxide can significantly improve the mechanical properties and wear resistance of rubber. Through cross-linking and reinforcement, graphene oxide can enhance the strength of rubber and improve its ability to withstand long-term wear. At the same time, it can also enhance the tensile and tear strength of rubber, making rubber products more durable during use. However, for non-polar rubbers, such as natural rubber, styrene-butadiene rubber, butadiene rubber, ethylene-propylene rubber, and butyl rubber, the dispersion of graphene oxide is more difficult due to the weak interfacial interaction between polar graphene oxide and the non-polar rubber matrix. In addition, weak interfacial interactions may lead to poor stress transfer in the rubber matrix and low graphene oxide reinforcement efficiency. Therefore, in order to obtain good dispersion of graphene oxide in the non-polar rubber matrix and achieve ideal performance, improving the interfacial interaction between graphene oxide and non-polar rubber remains a key and challenging problem to be solved.
[0004] Based on the above, adding porous starch and graphene oxide as fillers to natural rubber can synergistically improve the performance of rubber, but the technical disadvantages of each still need to be solved. Summary of the invention
[0005] The first aspect of the present invention provides a high mechanical property graphene rubber containing modified porous starch. The preparation raw materials include, by weight: 100 parts of natural rubber latex, 0.5-3 parts of modified porous starch, 0.4-1.5 parts of modified graphene oxide, 1-5 parts of gelling agent, 2-8 parts of zinc oxide, 1-4 parts of stearic acid, 1-2 parts of antioxidant, 0.5-2 parts of vulcanization accelerator, and 1-3 parts of vulcanizing agent.
[0006] In some embodiments, the solid content of the natural rubber latex is 60%.
[0007] In some embodiments, the preparation method of the modified porous starch includes: stirring and mixing the porous starch and water at 30-50° C., adjusting the pH value to 8-10, adding dodecyl succinic anhydride, reacting for 1-10 hours, adjusting the pH value to neutral with HCl aqueous solution, centrifuging, collecting the precipitate, washing and drying to obtain the modified porous starch.
[0008] In some embodiments, the mass ratio of the porous starch to dodecyl succinic anhydride is 1:(2-2.5), preferably 1:2.4.
[0009] The average fineness of the porous starch is 200 mesh, and the specific surface area of the porous starch is 11.34-35.40 m 2 / g.
[0010] The pH value is adjusted to 8-10 by using a NaOH aqueous solution, and the concentration of the NaOH aqueous solution is 0.5-2 mol / L, preferably 1 mol / L.
[0011] The concentration of the HCl aqueous solution is 0.5-2 mol / L, preferably 1 mol / L.
[0012] In some embodiments, the method for preparing the modified graphene oxide comprises: premixing graphene oxide and polyvinyl pyrrolidone in a ball mill, adding deionized water for ball milling, filtering and drying to obtain the modified graphene oxide.
[0013] In some embodiments, the mass ratio of graphene oxide to polyvinyl pyrrolidone is 1:(0.01-0.05), preferably 1:0.03.
[0014] In some embodiments, the graphene oxide has a particle size of 200-300 nm, an oxygen content of 25%-30%, a thickness of 0.5-2 nm, and the average molecular weight of the polyvinyl pyrrolidone is 360,000.
[0015] In some embodiments, the premixing time is 1-3 hours and the rotation speed is 100-200 rpm.
[0016] In some embodiments, the ball milling time is 18-36 hours and the rotation speed is 100-200 rpm.
[0017] In some embodiments, the gelling agent includes at least one of HDI copolymer bis-decyltetradeceth-20 and dibutyltin di(dodecylthio)eth-2.
[0018] In some embodiments, the antioxidant includes at least one of p-phenylenediamine and NN'-diphenyl-p-phenylenediamine.
[0019] In some embodiments, the vulcanization accelerator includes at least one of N-cyclohexyl-2-benzothiazole sulfonamide and dithiocarbamate.
[0020] In some embodiments, the vulcanizing agent is sulfur.
[0021] The second aspect of the present invention provides a method for preparing a graphene rubber with high mechanical properties containing modified porous starch, comprising the following steps:
[0022] S1. adding the modified porous starch to the suspension of modified graphene oxide, adding it dropwise to the natural rubber latex with stirring, continuing to add the gelling agent, washing and drying, to obtain a natural rubber composite material;
[0023] S2. The natural rubber composite material is mixed with zinc oxide, stearic acid, an antioxidant, a vulcanization accelerator, and a vulcanizing agent, and the mixture is allowed to stand and pressed to obtain a graphene rubber with high mechanical properties.
[0024] The third aspect of the present invention provides an application of high mechanical performance graphene rubber containing modified porous starch in the fields of automobiles, aerospace, and construction.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The modified porous starch prepared by esterification of dodecenyl succinate in the present invention can avoid self-agglomeration and has good dispersibility, thereby further enhancing its compatibility in natural rubber latex.
[0027] 2. The modified graphene oxide prepared by modification with polyvinyl pyrrolidone in the present invention can improve its compatibility in natural rubber latex, further improve its compatibility with modified starch, and has high stability in a variety of solvents, including water, ethanol, N-methylpyrrolidone, etc.
[0028] 3. The high mechanical performance graphene rubber prepared by the present invention significantly improves the mechanical properties of natural rubber under the synergistic effect of modified porous starch and modified graphene oxide, and further improves the processing stability of natural rubber. After various tests, it is significantly better than existing products. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The information of the substances in the present invention is as follows:
[0031] Natural rubber latex was purchased from Jinan Xinzheng Chemical Co., Ltd.
[0032] Porous starch was purchased from Liaoning Lida Biotechnology Co., Ltd.
[0033] Dodecylsuccinic anhydride, CAS: 26544-38-7.
[0034] Graphene oxide was purchased from Beijing Zhongke Leiming Co., Ltd.
[0035] Polyvinylpyrrolidone, CAS:9003-39-8.
[0036] NN'-diphenyl-p-phenylenediamine, CAS: 74-31-7.
[0037] N-Cyclohexyl-2-benzothiazolesulfonamide was purchased from Jinan Daen Pharmaceutical Technology Co., Ltd.
[0038] HDI copolymer bis-decyltetradecyl alcohol polyether-20 was purchased from Hubei Huada Fine Chemical Co., Ltd.
[0039] Example 1
[0040] The first aspect of the present embodiment provides a high mechanical property graphene rubber containing modified porous starch. The preparation raw materials include, by mass: 100 parts of natural rubber latex with a solid content of 60%, 1.5 parts of modified porous starch, 0.4 parts of modified graphene oxide, 3 parts of gelling agent, 3 parts of zinc oxide, 2 parts of stearic acid, 1.5 parts of antioxidant, 0.5 parts of vulcanization accelerator, and 2 parts of vulcanizing agent.
[0041] The preparation method of the modified porous starch comprises: stirring and mixing porous starch and water at 35° C., adjusting the pH value to 8 using a NaOH aqueous solution (with a concentration of 1 mol / L), adding dodecyl succinic anhydride, reacting for 4 hours, adjusting the pH value to neutral using a HCl aqueous solution (with a concentration of 1 mol / L), centrifuging, collecting precipitates, washing and drying to obtain the modified porous starch.
[0042] The average fineness of the porous starch is 200 mesh, and the specific surface area of the porous starch is 11.34-35.40 m 2 / g.
[0043] The mass ratio of porous starch to dodecylsuccinic anhydride is 1:2.4.
[0044] The mass of the water is 100 times that of the porous starch.
[0045] The preparation method of the modified graphene oxide comprises: premixing graphene oxide and polyvinyl pyrrolidone in a ball mill for 2 hours at a rotation speed of 150 rpm, adding deionized water for ball milling for 24 hours at a rotation speed of 180 rpm, filtering and drying to obtain the modified graphene oxide.
[0046] The mass ratio of the graphene oxide to polyvinyl pyrrolidone is 1:0.03.
[0047] The mass of the water is 100 times that of the graphene oxide.
[0048] The graphene oxide has a particle size of 200-300 nm, an oxygen content of 25%-30%, a thickness of 0.5-2 nm, distinct layers, and no obvious wrinkles. The average molecular weight of the polyvinyl pyrrolidone is 360,000.
[0049] The gelling agent is HDI copolymer bis-decyltetradecyl alcohol polyether-20, the antioxidant is NN'-diphenyl-p-phenylenediamine, the vulcanization accelerator is N-cyclohexyl-2-benzothiazole sulfonamide, and the vulcanizing agent is sulfur.
[0050] A second aspect of the present embodiment provides a method for preparing a graphene rubber with high mechanical properties containing modified porous starch, comprising the following steps:
[0051] S1. adding the modified porous starch to the suspension of modified graphene oxide, adding it dropwise to the natural rubber latex with stirring, continuing to add the gelling agent, washing and drying, to obtain a natural rubber composite material;
[0052] The preparation method of the modified graphene oxide suspension is as follows: 1 g of modified graphene oxide is mixed with 100 mL of water by ultrasonication to obtain the suspension.
[0053] S2. The natural rubber composite material is mixed with zinc oxide, stearic acid, an antioxidant, a vulcanization accelerator, and a vulcanizing agent, and the mixture is allowed to stand and pressed to obtain a graphene rubber with high mechanical properties.
[0054] Example 2
[0055] The specific implementation method of this embodiment is the same as that of Example 1, except that, by mass, the prepared raw materials include: 100 parts of natural rubber latex with a solid content of 60%, 1.5 parts of modified porous starch, 0.6 parts of modified graphene oxide, 3 parts of gelling agent, 3 parts of zinc oxide, 2 parts of stearic acid, 1.5 parts of antioxidant, 0.5 parts of vulcanization accelerator, and 2 parts of vulcanizing agent.
[0056] Example 3
[0057] The specific implementation method of this embodiment is the same as that of Example 1, except that, by mass, the prepared raw materials include: 100 parts of natural rubber latex with a solid content of 60%, 1.5 parts of modified porous starch, 0.8 parts of modified graphene oxide, 3 parts of gelling agent, 3 parts of zinc oxide, 2 parts of stearic acid, 1.5 parts of antioxidant, 0.5 parts of vulcanization accelerator, and 2 parts of vulcanizing agent.
[0058] Example 4
[0059] The specific implementation method of this embodiment is the same as that of Example 1, except that, by mass, the prepared raw materials include: 100 parts of natural rubber latex with a solid content of 60%, 1.5 parts of modified porous starch, 1 part of modified graphene oxide, 3 parts of gelling agent, 3 parts of zinc oxide, 2 parts of stearic acid, 1.5 parts of antioxidant, 0.5 parts of vulcanization accelerator, and 2 parts of vulcanizing agent.
[0060] Comparative Example 1
[0061] The specific implementation of this comparative example is the same as that of Example 3, except that the porous starch is not modified.
[0062] Comparative Example 2
[0063] The specific implementation of this comparative example is the same as that of Example 3, except that the modified graphene oxide is 0 parts.
[0064] Comparative Example 3
[0065] The specific implementation of this comparative example is the same as that of Example 3, except that the modified porous starch is 0 parts.
[0066] Comparative Example 4
[0067] The specific implementation of this comparative example is the same as that of Example 3, except that the mass ratio of porous starch to dodecyl succinic anhydride is 1:1.
[0068] Comparative Example 5
[0069] The specific implementation of this comparative example is the same as that of Example 3, except that the mass ratio of porous starch to dodecyl succinic anhydride is 1:4.
[0070] Comparative Example 6
[0071] The specific implementation of this comparative example is the same as that of Example 3, except that maleic anhydride is used to replace dodecyl succinic anhydride.
[0072] Comparative Example 7
[0073] The specific implementation of this comparative example is the same as that of Example 3, except that the mass ratio of the graphene oxide to polyvinyl pyrrolidone is 1:0.08.
[0074] Comparative Example 8
[0075] The specific implementation of this comparative example is the same as that of Example 3, except that the graphene oxide has a diameter of 0.3-3 μm, a thickness of 0.55-1.2 nm, 1-5 layers, a purity of 99.9 wt %, and is purchased from Zhongke Leiming (Beijing) Technology Co., Ltd., model CNT901, and the average molecular weight of the polyvinyl pyrrolidone is 400,000.
[0076] Comparative Example 9
[0077] The specific implementation of this comparative example is the same as that of Example 3, except that hydroxycellulose is used to replace polyvinyl pyrrolidone.
[0078] Comparative Example 10
[0079] The specific implementation method of this comparative example is the same as that of Example 3, except that, by mass, the prepared raw materials include: 100 parts of natural rubber latex with a solid content of 60%, 5 parts of modified porous starch, 3 parts of modified graphene oxide, 3 parts of gelling agent, 3 parts of zinc oxide, 2 parts of stearic acid, 1.5 parts of antioxidant, 0.5 parts of vulcanization accelerator, and 2 parts of vulcanizing agent.
[0080] Performance Testing
[0081] The graphene rubbers with high mechanical properties prepared in the above examples and comparative examples were subjected to the following tests.
[0082] (1) Tensile properties:
[0083] The test was carried out on a Shenzhen Sansi CMT4254 electronic universal tensile testing machine according to GB / T528-2009 standard, with a tensile rate of 500 mm / min. The modulus at 100% elongation (M100), modulus at 300% elongation (M300), tensile strength, and elongation at break of the rubber were recorded, and the results are recorded in Table 1.
[0084] (2) Tear performance:
[0085] The test was carried out on a Shenzhen Sansi CMT4254 electronic universal tensile testing machine according to GB / T529-2009 standard at a speed of 500 mm / min. The tear strength of the rubber was recorded and the results are recorded in Table 1.
[0086] (3) Moisture resistance:
[0087] The graphene rubber with high mechanical properties prepared in the above examples and comparative examples was placed at 30° C. and 80% humidity for 7 days with the same mass and volume, and then the mechanical properties were tested. The results are recorded in Table 2.
[0088] Table 1
[0089]
[0090] Table 2
[0091]
[0092]
[0093] It can be seen from the above data that the modified graphene oxide prepared by the present invention not only improves its compatibility in natural rubber latex, but also improves its compatibility with modified starch, and has high stability in a variety of solvents, including water, ethanol, N-methylpyrrolidone, etc. This is because defective graphene oxide is obtained after ball milling, and the defects at the edges of graphene oxide contain many active unsaturated bonds, which are easy to combine with other surfactants. In the ball milling experiment, the long molecular chain of polyvinyl pyrrolidone as an amphiphilic polymer breaks under the long-term action of shear force, resulting in the combination of graphene edges and fragmented polyvinyl pyrrolidone molecules. These broken polyvinyl pyrrolidone molecules can largely avoid the agglomeration of graphene oxide.
[0094] As can be seen from Table 1, the graphene rubber with high mechanical properties prepared by the present invention complements each other through the filling and reinforcing effect of modified porous starch and the mechanical reinforcing effect of modified graphene oxide, and the two work synergistically to improve the comprehensive mechanical properties of natural rubber. In addition, the adsorption of modified porous starch and the stability of modified graphene oxide improve the processing stability of natural rubber to a certain extent. Although the performance of rubber is improved by single modified porous starch and modified graphene oxide, the improvement effect is far worse than the effect of the composite of the two materials, and the two are not mutually balanced to affect the performance. As can be seen from Table 2, the graphene rubber with high mechanical properties prepared by the present invention still maintains strong mechanical properties under the conditions of 30°C and 80% humidity. The synergistic effect of the two reduces the water absorption rate, and the rubber does not suffer a large loss of mechanical properties.
[0095] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high mechanical performance graphene rubber containing modified porous starch, characterized in that: The raw materials include, by weight: 100 parts of natural rubber latex, 0.5-3 parts of modified porous starch, 0.4-1.5 parts of modified graphene oxide, 1-5 parts of gelling agent, 2-8 parts of zinc oxide, 1-4 parts of stearic acid, 1-2 parts of antioxidant, 0.5-2 parts of vulcanization accelerator and 1-3 parts of vulcanizing agent.
2. The high mechanical performance graphene rubber according to claim 1, characterized in that: The preparation method of the modified porous starch comprises: stirring and mixing the porous starch and water at 30-50° C., adjusting the pH value to 8-10, adding dodecyl succinic anhydride, reacting for 1-10 hours, adjusting the pH value to neutral with HCl aqueous solution, centrifuging, collecting the precipitate, washing and drying to obtain the modified porous starch.
3. The high mechanical performance graphene rubber according to claim 2, characterized in that: The mass ratio of the porous starch to dodecyl succinic anhydride is 1:(2-2.5), the average fineness of the porous starch is 200 mesh, and the specific surface area of the porous starch is 11.34-35.40 m 2 / g.
4. The graphene rubber with high mechanical properties according to claim 1, characterized in that: The preparation method of the modified graphene oxide comprises: premixing graphene oxide and polyvinyl pyrrolidone in a ball mill, adding deionized water for ball milling, filtering and drying to obtain the modified graphene oxide.
5. The graphene rubber with high mechanical properties according to claim 4, characterized in that: The mass ratio of the graphene oxide to polyvinyl pyrrolidone is 1:(0.01-0.05).
6. The graphene rubber with high mechanical properties according to claim 5, characterized in that: The graphene oxide has a particle size of 200-300 nm, an oxygen content of 25%-30%, a thickness of 0.5-2 nm, and the average molecular weight of the polyvinyl pyrrolidone is 360,000.
7. The graphene rubber with high mechanical properties according to claim 6, characterized in that: The premixing time is 1-3 hours, and the rotation speed is 100-200 rpm.
8. The graphene rubber with high mechanical properties according to claim 7, characterized in that: The ball milling time is 18-36 hours, and the rotation speed is 100-200 rpm.
9. A method for preparing graphene rubber with high mechanical properties containing modified porous starch according to any one of claims 1 to 8, characterized in that: The steps include: S1. adding the modified porous starch to the suspension of modified graphene oxide, adding it dropwise to the natural rubber latex with stirring, continuing to add the gelling agent, washing and drying, to obtain a natural rubber composite material; S2. The natural rubber composite material is mixed with zinc oxide, stearic acid, an antioxidant, a vulcanization accelerator, and a vulcanizing agent, and the mixture is allowed to stand and pressed to obtain a graphene rubber with high mechanical properties.
10. Application of high mechanical performance graphene rubber containing modified porous starch in the fields of automobile, aerospace, and construction.