Low-cost rubber for blasting as well as preparation method and application of low-cost rubber

By optimizing the formula and process of recycled rubber and adding specific additives and fibers, the weather resistance and aging resistance of rubber are improved, the problem of insufficient performance of recycled rubber is solved, and a low-cost, high-performance rubber isolator for blasting is realized, which alleviates the The problem of natural rubber shortage and environmental pollution has been solved.

CN118725436AActive Publication Date: 2024-10-01JIANGXI DEXING YICUN IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411144928.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-01
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Recycled rubber has poor weather resistance, flex resistance, compression permanent deformation, tensile resistance and tear resistance, which makes rubber isolators used for blasting easy to wear and age, making it difficult to meet the performance requirements of mine blasting.

Method used

Using fully recycled rubber as raw material, through optimizing the formula and process, adding white carbon black, nano-calcium carbonate, zinc oxide, modified polyester fiber, paraffin, antioxidants and accelerators to improve the physical and mechanical properties and processing performance of the rubber, and improve Its weather resistance, aging resistance and tear resistance.

Benefits of technology

Low-cost rubber for blasting with excellent performance is obtained, which is suitable for rubber isolators for mine blasting. It alleviates the shortage of natural rubber, reduces environmental pollution, and has extensive economic and social value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of rubber, and particularly relates to low-cost rubber for blasting as well as a preparation method and application thereof. The rubber formula comprises the following raw materials in parts by weight: 100 parts of tread reclaimed rubber, 2-4 parts of white carbon black, 20-40 parts of nano calcium carbonate, 2-4 parts of zinc oxide, 2-3 parts of modified polyester fibers, 0.5-1.2 parts of paraffin, 2-4 parts of stearic acid, 1-2 parts of an anti-aging agent, 0.5-1.7 parts of an accelerant and 1-3 parts of sulfur. According to the rubber for blasting, the regenerated rubber is completely used as the raw material, the auxiliary ingredients and the proportion are optimized, and the obtained rubber is excellent in comprehensive performance and low in cost, can be used for manufacturing rubber isolators for mine blasting, can relieve shortage of natural rubber, fully utilizes renewable resources and reduces environmental pollution, and has wide economic value and social value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber, and in particular relates to a low-cost blasting rubber and a preparation method and application thereof. Background Art

[0002] The natural degradation process of rubber products is very long. Waste rubber causes black pollution which is more difficult to deal with than plastic pollution (white pollution). At the same time, it seriously wastes precious rubber resources. Therefore, carefully and properly handling waste rubber has extremely far-reaching practical significance for making full use of renewable resources, reducing environmental pollution and improving the living environment.

[0003] Recycled rubber is a kind of rubber that is processed from waste rubber products, has a certain degree of plasticity and can be reused. Recycled rubber is an important raw material for the rubber industry. On the one hand, it can replace rubber, alleviate the serious shortage of natural rubber, and is an important measure to solve the environmental pollution caused by waste rubber; on the other hand, recycled rubber is cheap, and recycled rubber products have huge cost advantages. Rubber isolators for blasting can improve the blasting effect and efficiency. Rubber isolators for blasting are disposable products. If rubber isolators can be made of recycled rubber, it is not only environmentally friendly but also low in cost. However, recycled rubber has some defects. Its weather resistance, flexure, compression permanent deformation, tensile and tear resistance are poor, and recycled rubber products may be easy to wear and age due to insufficient strength. Therefore, it is of great significance to develop a technology that can prepare rubber isolators for blasting with excellent performance using only recycled rubber by optimizing the raw material ratio. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a low-cost blasting rubber and a preparation method and application thereof. The blasting rubber uses fully recycled rubber as raw material, and the obtained rubber has excellent comprehensive performance and low cost. It is used to make rubber isolators for mine blasting, which can alleviate the shortage of natural rubber, make full use of recycled resources, and reduce environmental pollution. It has broad economic and social value.

[0005] To achieve the above object, the present invention provides a low-cost blasting rubber, wherein the rubber formula comprises the following raw materials in parts by weight: 100 parts of tread reclaimed rubber, 2-4 parts of white carbon black, 20-40 parts of nano calcium carbonate, 2-4 parts of zinc oxide, 2-3 parts of modified polyester fiber, 0.5-1.2 parts of paraffin, 2-4 parts of stearic acid, 1-2 parts of antioxidant, 0.5-1.7 parts of accelerator, and 1-3 parts of sulfur.

[0006] In this technical solution, tread reclaimed rubber is used as raw material. By optimizing the auxiliary agent composition, the weather resistance, aging resistance, flexure resistance, tensile and tear resistance of tread reclaimed rubber can be effectively improved, and the rubber has good resilience and wear resistance. Among them, by adding a small amount of white carbon black, the physical and mechanical properties, wear resistance, and flexure crack resistance of rubber products can be improved; by adding a certain amount of nano calcium carbonate, the dispersion is good, the wear resistance, tear resistance and aging resistance of rubber products are improved, and the processing performance of rubber is improved; by adding zinc oxide as an active agent, the vulcanization efficiency can be improved, the amount of accelerator can be reduced, and as a reinforcing agent, the rubber corrosion resistance and aging resistance can be improved, and a certain elasticity can be added; by adding a certain amount of modified polyester fiber, the impact resistance and flexure of rubber can be increased, and the strength, resilience and stability are good; by adding paraffin, a protective layer can be formed on the rubber surface to prevent ozone cracking and improve aging resistance; by adding stearic acid, the processing of the rubber can be improved, the dispersion of raw materials can be promoted, and it can synergize with zinc oxide to promote vulcanization.

[0007] Furthermore, in the above technical solution, the preparation method of the modified polyester fiber is: after the polyester fiber is crushed, it is placed in a water-soluble epoxy resin solution, an appropriate amount of sodium hydroxide solution is added, and it is immersed in ultrasonic conditions for 50-80 minutes, washed and dried, and then immersed in phenolic resin latex for 15-20 minutes, dried and cured to obtain the modified polyester fiber. Polyester fiber has high breaking strength, small elongation under fixed load, small deformation, good impact resistance and heat resistance, low water absorption, etc., but it is difficult to bond with rubber. In the technical scheme, the polyester fiber is modified and, under certain conditions, first combined with an epoxy resin solution, so that the epoxy group reacts with the ester group, hydroxyl group, carboxyl group and other active groups on the surface of the polyester fiber to form a stable chemical bond, and the hydroxyl group and the carbonyl group on the surface of the polyester fiber form a hydrogen bond, etc., which can increase the adhesion between the polyester fiber and the resin; then the polyester fiber is further treated with a phenolic resin latex, and the active functional groups such as the phenolic hydroxyl group and the aldehyde group in the phenolic resin molecule are further reacted with the hydroxyl group on the surface of the polyester fiber, and can be filled into the fiber micropores, thereby improving the fiber strength and wear resistance, while further improving the adhesion and stability between the polyester fiber and the rubber.

[0008] Furthermore, in the above technical solution, the length of the polyester fiber is less than 10 mm.

[0009] Furthermore, in the above technical solution, the concentration of epoxy resin in the water-soluble epoxy resin solution is 50-80 g / L; the ultrasonic frequency is 10-15 kHz; and the immersion temperature is 70-85°C.

[0010] Furthermore, in the above technical solution, the mass ratio of phenolic resin: water: latex in the phenolic resin latex is 1-4:15-25:15-30.

[0011] Furthermore, in the above technical solution, the particle size of the white carbon black is 150-200nm, and its specific surface area is 20-30m 2 / g; the antioxidant is a mixture of antioxidant D (N-phenyl-2-naphthylamine) and antioxidant 2246 (antioxidant 2246) in a mass ratio of 1:1-3. In this technical solution, ultra-low specific surface area white carbon black is selected as a reinforcing agent, which can not only replace ordinary carbon black, but also improve processing performance and resistance to flexion cracking. Antioxidant D is an amine antioxidant, which has heat resistance, oxidation resistance, ozone resistance, and protective effects on copper ions and flexibility, but it is easy to change color when exposed to light; antioxidant 2246 is a phenolic antioxidant, which has the characteristics of no discoloration and no pollution, and has good protective efficiency against heat, oxygen, metal ion aging, sunlight aging, etc. The present invention combines the advantages of both and uses two antioxidants in combination, which can greatly improve the weather resistance and aging resistance of rubber and extend the service life of rubber.

[0012] Furthermore, in the above technical solution, the accelerator is a mixture of accelerator DM (dibenzothiazyl disulfide) and accelerator TMTD (tetramethylthiuram disulfide) in a mass ratio of 0.5-1.5: 0.05-0.15. Accelerator DM is a thiazole accelerator, and accelerator TMTD is a thiuram accelerator. The combination of the two can improve the activity, thereby improving the vulcanization efficiency, improving the mechanical properties of the vulcanized rubber, and the dosage is small.

[0013] The present invention also provides a method for preparing low-cost blasting rubber, comprising the following steps: (1) Weigh each raw material according to the weight of each component in the formula and set aside; (2) placing the tread regenerated rubber into a steam explosion tank for explosion treatment to obtain pre-treated tread regenerated rubber; (3) Set the roller temperature of the mixing mill to 45-50°C. When the roller temperature exceeds 50°C, pass water at 20-25°C to lower the roller temperature. Then put the pre-treated tread reclaimed rubber into the mixing mill for 3-4 minutes, and pass it 4-6 times during the process. (4) Add paraffin wax and stearic acid into an open mixer and mix for 3-4 minutes; (5) Add the modified polyester fiber into an open mill and mix for 5-6 minutes; (6) Add antioxidant, zinc oxide and accelerator into the mixing mill and mix for 2-3 minutes; (7) Add nano calcium carbonate and carbon black into an open mill and mix for 3-4 minutes; (8) Add sulfur to the open mixing mill and mix for 6-7 minutes, during which time, make triangle bags 3-4 times to obtain a mixed rubber; (9) Thinly pass the mixed rubber 3-5 times and cut into sheets.

[0014] Furthermore, in step (2) of the above technical solution, the steam explosion conditions are: pressure 6-8MPa, and the pressure is maintained for 120-150s. In this technical solution, the countertop recycled rubber is pre-treated by steam explosion. During the steam explosion process, the high-temperature steam can evenly preheat the rubber particles, so that the rubber liquid maintains a high viscosity when it is melted, thereby increasing the rubber content of the rubber product and enhancing the rubber resilience; at the same time, it can improve the internal structure of the rubber, reduce cracking and peeling caused by uneven heating or stress concentration, and improve the durability of the rubber product.

[0015] The present invention also provides an application of the low-cost blasting rubber in a rubber isolator for mine blasting.

[0016] The present invention has the following beneficial effects: The present invention uses full tread recycled rubber as raw material, and by optimizing the ratio of auxiliary ingredients and the preparation process, can effectively improve the weather resistance, aging resistance, flexure resistance, tensile and tear resistance of the tread recycled rubber, has good resilience and wear resistance, and greatly reduces the cost; using it to prepare rubber isolators for mine blasting not only has excellent performance, but also can alleviate the serious shortage of natural rubber. It is an important measure to solve the environmental pollution of waste rubber, has extremely far-reaching practical significance for making full use of renewable resources, reducing environmental pollution, and improving the living environment, and has broad economic value and social value. DETAILED DESCRIPTION

[0017] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials involved in the following examples are common commercial products and can be purchased from the market unless otherwise specified.

[0018] The preparation processes not specifically described in the present invention are all conventional processes.

[0019] The present invention is described in further detail below in conjunction with embodiments: Example 1 A method for preparing low-cost blasting rubber comprises the following steps: (1) Weigh the raw materials according to the weight of each component in the formula: 100 parts of tread reclaimed rubber, 2 parts of white carbon black, 40 parts of nano calcium carbonate, 2 parts of zinc oxide, 2 parts of modified polyester fiber, 1.2 parts of paraffin wax, 2 parts of stearic acid, 1 part of antioxidant, 1.7 parts of accelerator, and 1 part of sulfur; the particle size of white carbon black is 150-200nm, and its specific surface area is 20m 2 / g; the antioxidant is a mixture of antioxidant D and antioxidant 2246 in a mass ratio of 1:1; the accelerator is a mixture of accelerator DM and accelerator TMTD in a mass ratio of 0.5:0.05; the modification method of the modified polyester fiber is as follows: after the polyester fiber is crushed to a length of less than 10 mm, it is put into a solution with an epoxy resin concentration of 50 g / L, an appropriate amount of 5% hydroxide solution is added to make the solution alkaline, and the solution is immersed in an ultrasonic condition of a temperature of 85°C and a frequency of 15 kHz for 50 minutes, after washing and drying, it is immersed in phenolic resin latex (the mass ratio of phenolic resin: water: latex is 1:15:15) for 20 minutes, dried and cured to obtain the modified polyester fiber.

[0020] (2) placing the tread regenerated rubber in a steam explosion tank at a pressure of 6 MPa for 150 seconds for explosion treatment to obtain pretreated tread regenerated rubber; (3) Set the roller temperature of the open mill to 45-50°C. When the roller temperature exceeds 50°C, pass water at 20-25°C to lower the roller temperature. Then put the pre-treated tread reclaimed rubber into the open mill for 3 minutes, during which time it is thinly passed 6 times. (4) Add paraffin wax and stearic acid into an open mixer and mix for 3 minutes; (5) Add the modified polyester fiber into an open mill and mix for 5 minutes; (6) Add antioxidant, zinc oxide and accelerator into an open mill and mix for 2 minutes; (7) Add nano calcium carbonate and carbon black into an open mill and mix for 3 minutes; (8) Add sulfur to the mixing mill and mix for 7 minutes, during which time the mixture is triangularly packaged 4 times to obtain a mixed rubber; (9) Thinly pass the mixed rubber through 5 times and roll it into sheets.

[0021] Example 2 A method for preparing low-cost blasting rubber comprises the following steps: (1) Weigh the raw materials according to the weight of each component in the formula: 100 parts of tread reclaimed rubber, 3 parts of white carbon black, 30 parts of nano calcium carbonate, 3 parts of zinc oxide, 2.5 parts of modified polyester fiber, 1 part of paraffin, 3 parts of stearic acid, 1.5 parts of antioxidant, 1 part of accelerator, and 2 parts of sulfur; among which, the particle size of white carbon black is 150-200nm, and its specific surface area is 20-30m 2 / g; the antioxidant is a mixture of antioxidant D and antioxidant 2246 in a mass ratio of 1:2; the accelerator is a mixture of accelerator DM and accelerator TMTD in a mass ratio of 1:0.15; the modification method of the modified polyester fiber is as follows: after the polyester fiber is crushed to a length of less than 10 mm, it is put into a solution with an epoxy resin concentration of 60 g / L, an appropriate amount of 5% hydroxide solution is added to make the solution alkaline, and the solution is immersed for 60 minutes under ultrasonic conditions of a temperature of 80°C and a frequency of 12 kHz, after washing and drying, it is immersed in phenolic resin latex (the mass ratio of phenolic resin: water: latex is 3:20:20) for 15-20 minutes, dried and cured to obtain the modified polyester fiber.

[0022] (2) placing the tread regenerated rubber in a steam explosion tank at a pressure of 7 MPa for 130 seconds to perform explosion treatment, thereby obtaining pre-treated tread regenerated rubber; (3) Set the roller temperature of the mixing mill to 45-50°C. When the roller temperature exceeds 50°C, pass water at 20-25°C to lower the roller temperature. Then put the pre-treated tread reclaimed rubber into the mixing mill and mix for 3.5 minutes, during which time the water is passed through the mixing mill 5 times. (4) Add paraffin wax and stearic acid into an open mixer and mix for 3.5 minutes; (5) Add the modified polyester fiber into an open mill and mix for 5.5 minutes; (6) Add antioxidant, zinc oxide and accelerator into an open mill and mix for 2.5 minutes; (7) Add nano calcium carbonate and carbon black into an open mixer and mix for 3.5 minutes; (8) Add sulfur to the mixing mill and mix for 6.5 min. During the mixing, make a triangle bag three times to obtain a mixed rubber; (9) Pass the mixed rubber through 4 thin passes and roll into sheets.

[0023] Example 3 A method for preparing low-cost blasting rubber comprises the following steps: (1) Weigh the raw materials according to the weight of each component in the formula: 100 parts of tread reclaimed rubber, 4 parts of white carbon black, 20 parts of nano calcium carbonate, 4 parts of zinc oxide, 3 parts of modified polyester fiber, 0.5 parts of paraffin, 4 parts of stearic acid, 2 parts of antioxidant, 0.5 parts of accelerator, and 3 parts of sulfur; among which, the particle size of white carbon black is 150-200nm, and its specific surface area is 20-30m 2 / g; the antioxidant is a mixture of antioxidant D and antioxidant 2246 in a mass ratio of 1:3; the accelerator is a mixture of accelerator DM and accelerator TMTD in a mass ratio of 1.5:0.1; the modification method of the modified polyester fiber is as follows: after the polyester fiber is crushed to a length of less than 10 mm, it is put into a solution with an epoxy resin concentration of 80 g / L, an appropriate amount of 5% hydroxide solution is added to make the solution alkaline, and the solution is immersed for 80 minutes under ultrasonic conditions of a temperature of 70°C and a frequency of 10 kHz, after washing and drying, it is immersed in phenolic resin latex (the mass ratio of phenolic resin: water: latex is 4:25:30) for 15 minutes, dried and cured to obtain the modified polyester fiber.

[0024] (2) placing the tread reclaimed rubber in a steam explosion tank at a pressure of 8 MPa for 120 seconds to perform explosion treatment, thereby obtaining pre-treated tread reclaimed rubber; (3) Set the roller temperature of the mixing mill to 45-50°C. When the roller temperature exceeds 50°C, pass water at 20-25°C to lower the roller temperature. Then put the pre-treated tread reclaimed rubber into the mixing mill for 4 minutes, and pass it through the mixing mill 4 times. (4) Add paraffin wax and stearic acid into an open mixer and mix for 4 minutes; (5) Add the modified polyester fiber into an open mill and mix for 6 minutes; (6) Add antioxidant, zinc oxide and accelerator into an open mill and mix for 3 minutes; (7) Add nano calcium carbonate and carbon black into an open mill and mix for 4 minutes; (8) Add sulfur to the open mixing mill and mix for 6 minutes, during which time the mixture is triangularly packaged 3 times to obtain a mixed rubber; (9) Thinly pass the mixed rubber through 3 times and roll it into sheets.

[0025] Comparative Example 1 A method for preparing low-cost blasting rubber is disclosed, which differs from Example 2 in that ordinary polyester fiber is used, and the rest is the same as Example 2.

[0026] Comparative Example 2 A method for preparing low-cost blasting rubber is disclosed, which differs from Example 2 in that modified polyester fiber is not added, and the rest is the same as Example 2.

[0027] Comparative Example 3 A method for preparing low-cost blasting rubber, which differs from Example 2 in that ordinary carbon black is used, and the specific surface area is 150m 2 / g, and the rest is the same as in Example 2.

[0028] Comparative Example 4 A method for preparing low-cost blasting rubber, which differs from Example 2 in that the antioxidant is a single antioxidant D, and the rest is the same as Example 2.

[0029] Comparative Example 5 A method for preparing low-cost blasting rubber, which differs from Example 2 in that the antioxidant is a single antioxidant 2246, and the rest is the same as Example 2.

[0030] Comparative Example 6 A method for preparing low-cost blasting rubber, which is different from Example 2 in that the accelerator is a single accelerator DM, and the rest is the same as Example 2.

[0031] Comparative Example 7 A method for preparing low-cost blasting rubber is different from Example 2 in that the accelerator is a single accelerator TMTD, and the rest is the same as Example 2.

[0032] Comparative Example 8 A method for preparing low-cost blasting rubber is disclosed, which differs from Example 2 in that the method does not include step (2), and the rest is the same as Example 2.

[0033] The mixed rubbers obtained in Examples 1-3 and Comparative Examples 1-8 were vulcanized into 2.0 mm sheets using a flat plate vulcanizer at a vulcanization temperature of 143° C. for 3 min, and then tested for relevant properties such as hardness (GB / T531), mechanical properties (including tensile strength, elongation at break, tear strength) (GB / T 528), resilience (GB / T 1681), aging resistance (GB3512), compression set (GB / T 7759), wear resistance (GB / T1689), and ozone resistance (GB / T7762). The results are shown in Tables 1 and 2.

[0034] Table 1 Performance test results of Examples 1-3

[0035] Table 2 Performance test results of comparative examples 1-8

[0036] It can be seen from the results in Table 1 that the rubber compound obtained by the formula and preparation method of the present invention has excellent hardness, tensile strength, resilience, compression permanent deformation, wear resistance and weather resistance and aging resistance, and has excellent overall performance, and can be used to make rubber isolators for mine blasting.

[0037] From the results in Table 2, it can be seen that the performance of Comparative Example 1 was affected by the use of ordinary polyester fiber, which may be due to its poor bonding with the tread reclaimed rubber, which affected its overall performance; in Comparative Example 2, no polyester fiber was added, and its overall performance was worse, especially the poor resilience; in Comparative Example 3, ordinary high specific surface area carbon black was used, which also had a reinforcing effect, but its effect was not as good as that of low specific surface area white carbon black; in Comparative Examples 4-5, only a single antioxidant D or antioxidant 2246 was used, and its anti-aging and ozone performances were reduced, indicating that the two had a synergistic effect; in Comparative Examples 6-7, only a single accelerator DM or accelerator TMTD was used, and its overall performance was also reduced; in Comparative Example 8, the tread reclaimed rubber was not pre-treated by steam explosion during the preparation process, and its overall performance was greatly reduced, indicating that steam explosion pre-treatment of the tread reclaimed rubber before mixing can improve rubber resilience, aging resistance, cracking resistance and other properties.

[0038] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A low-cost blasting rubber, characterized in that: The rubber formula includes the following raw materials in parts by weight: 100 parts of tread reclaimed rubber, 2-4 parts of white carbon black, 20-40 parts of nano calcium carbonate, 2-4 parts of zinc oxide, 2-3 parts of modified polyester fiber, 0.5-1.2 parts of paraffin, 2-4 parts of stearic acid, 1-2 parts of antioxidant, 0.5-1.7 parts of accelerator, and 1-3 parts of sulfur.

2. A low-cost blasting rubber according to claim 1, characterized in that: The preparation method of the modified polyester fiber is as follows: the polyester fiber is crushed, put into a water-soluble epoxy resin solution, an appropriate amount of sodium hydroxide solution is added, and it is immersed for 50-80 minutes under ultrasonic conditions, washed and dried, and then immersed in phenolic resin latex for 15-20 minutes, dried and cured to obtain the modified polyester fiber.

3. A low-cost blasting rubber according to claim 2, characterized in that: The polyester fiber has a length of less than 10 mm.

4. A low-cost blasting rubber according to claim 2, characterized in that: The concentration of the epoxy resin in the water-soluble epoxy resin solution is 50-80 g / L; the ultrasonic frequency is 10-15 kHz; and the immersion temperature is 70-85° C.

5. A low-cost blasting rubber according to claim 2, characterized in that: The mass ratio of phenolic resin: water: latex in the phenolic resin latex is 1-4:15-25:15-30.

6. The low-cost blasting rubber according to claim 1, characterized in that: The particle size of the white carbon black is 150-200nm, and its specific surface area is 20-30m 2 / g; the antioxidant is a mixture of antioxidant D and antioxidant 2246 in a mass ratio of 1:1-3.

7. The low-cost blasting rubber according to claim 1, characterized in that: The accelerator is a mixture of accelerator DM and accelerator TT in a mass ratio of 0.5-1.5: 0.05-0.

15.

8. A method for preparing low-cost blasting rubber according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Weigh each raw material according to the weight of each component in the formula and set aside; (2) placing the tread regenerated rubber into a steam explosion tank for explosion treatment to obtain pre-treated tread regenerated rubber; (3) Set the roller temperature of the mixing mill to 45-50°C. When the roller temperature exceeds 50°C, pass water at 20-25°C to lower the roller temperature. Then put the pre-treated tread reclaimed rubber into the mixing mill for 3-4 minutes, and pass it 4-6 times during the process. (4) Add paraffin wax and stearic acid into an open mixer and mix for 3-4 minutes; (5) Add the modified polyester fiber into an open mill and mix for 5-6 minutes; (6) Add antioxidant, zinc oxide and accelerator into the mixing mill and mix for 2-3 minutes; (7) Add nano calcium carbonate and carbon black into an open mill and mix for 3-4 minutes; (8) Add sulfur to the open mixing mill and mix for 6-7 minutes, during which time, make triangle bags 3-4 times to obtain a mixed rubber; (9) Thinly pass the mixed rubber 3-5 times and cut into sheets.

9. The preparation method according to claim 8, characterized in that: In step (2), the conditions for steam explosion are: pressure 6-8 MPa, and pressure maintenance time 120-150 s.

10. Use of the low-cost blasting rubber according to any one of claims 1 to 7 or the low-cost blasting rubber prepared by the preparation method according to any one of claims 8 to 9 in a rubber isolator for mine blasting.

Citation Information

Patent Citations

  • Aqueous dipping composition for polyester rubber pipe yarns, and preparation method thereof

    CN103757910A

  • Waste tire rubber powder / aramid pulp pre-dispersion and preparation method thereof

    CN107814951A

  • Recoverable environmental protection type material of rubber, and application

    CN1872907A

  • Polyester fiber material that has improved adhesion with rubber, and method for producing the same

    JP2006274530A

  • Adhesive composition for organic fiber, method of treating organic fiber, organic fiber, and tire

    JP2019178294A