Ethylene-propylene-diene monomer rubber compound

By using materials such as polyethylene terephthalate and polycarbonate in the EPDM rubber compound, the problem of reduced adhesive performance caused by the denaturation of polytetrahydrofuran ether glycol at high temperatures is solved, and the rubber is realized at high temperatures. stable performance and extended service life.

CN118725474APending Publication Date: 2024-10-01ANHUI DINGLIAN POLYMER MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410840719.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing EPDM rubber compound turns into a transparent liquid due to polytetrahydrofuran ether glycol at high temperatures, resulting in a decrease in the material's molecular adhesion properties and affecting the service life of the rubber.

Method used

Materials such as polyethylene terephthalate and polycarbonate are used to replace polytetrahydrofuran ether glycol. By adjusting the formula and process steps, the rubber can maintain its antistatic function and mechanical properties at high temperatures and extend its service life.

Benefits of technology

It maintains the antistatic function and mechanical properties of rubber at high temperatures, extends the service life of rubber, and improves electrical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an ethylene propylene diene monomer rubber compound, which is prepared from the following ingredients in parts by weight: 18 to 32 parts of ethylene propylene diene monomer rubber base materials, 5 to 15 parts of chloroprene rubber, 6 to 16 parts of polyethylene terephthalate, 3 to 14 parts of polyvinyl alcohol, 54 to 65 parts of polyisobutene and 3 to 14 parts of polycarbonate. By adding poly (p-polycarbonate) into mixed particles, the rubber can still keep a relatively strong antistatic function at high temperature, and meanwhile, the added chloroprene rubber and polyisobutene can improve the mechanical property of the rubber under the condition of improving the acid, alkali and salt corrosion resistance of the rubber, so that the service life of the rubber is greatly prolonged; and by filling the polyethylene terephthalate into the mixed particles, the rubber can still keep a relatively strong antistatic function at a high temperature of 120 DEG C, so that the electrical properties of the ethylene propylene diene monomer rubber compound are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of EPDM rubber production, in particular to an EPDM rubber compound. Background Art

[0002] EPDM is a copolymer of ethylene, propylene and a small amount of non-conjugated dienes. It is a type of ethylene-propylene rubber, represented by EPDM. Because its main chain is composed of chemically stable saturated hydrocarbons and only contains unsaturated double bonds in the side chains, it has excellent aging resistance such as ozone resistance, heat resistance, and weather resistance. It can be widely used in automotive parts, building waterproof materials, wire and cable sheaths, heat-resistant hoses, tapes, automotive seals and other fields.

[0003] Rubber mix refers to the uncrosslinked and fluid rubber material obtained by mixing compounding agents with raw rubber in block, granular or powder form. The rubber material obtained by mixing raw rubber or plasticized rubber with compounding agents in a rubber mixer according to the formula is called rubber mix.

[0004] In the prior art, the publication number "CN102952478A" discloses a filter adhesive film obtained by mixing chloroprene rubber and EPDM rubber, which is made of raw materials such as chloroprene rubber CR121, styrene, EPDM rubber, 2.4.6-tris(dimethylaminomethyl)phenol, polyvinyl alcohol, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, polyisobutylene, polytetrahydrofuran ether glycol, and modified tree ash. The present invention mixes chloroprene rubber and EPDM rubber, and adds compound powder as a filler, so that the present invention has good temperature resistance, high shear strength, excellent electrical insulation and aging resistance, and the adhesive film has a smooth surface, good toughness, and good anti-seismic effect after curing.

[0005] However, the existing technology still has major deficiencies, such as:

[0006] In the above device and the prior art, polytetramethylene ether glycol is a chemical substance, a white waxy solid, easily soluble in alcohols, esters, ketones, aromatic hydrocarbons and chlorinated hydrocarbons, and insoluble in aliphatic hydrocarbons and water. When the molecular weight increases, the solubility decreases. The addition of modified tree ash materials can enhance the electrical insulation of rubber materials, but when the temperature exceeds room temperature, polytetramethylene ether glycol will become a transparent liquid, which reduces the bonding effect between the modified tree ash and the remaining materials, thereby reducing the molecular bonding performance of the rubber internal materials and affecting the service life of the rubber. Summary of the invention

[0007] The object of the present invention is to provide an EPDM rubber compound to solve the problems raised in the above background technology.

[0008] To achieve the above-mentioned purpose, the present invention provides the following technical solution: an EPDM rubber compound, comprising the following components counted by weight: 18-32 parts of EPDM rubber base material, 5-15 parts of chloroprene rubber, 6-16 parts of polyethylene terephthalate, 3-14 parts of polyvinyl alcohol, 54-65 parts of polyisobutylene, and 3-14 parts of polycarbonate.

[0009] Preferably, the EPDM base material is 19-31 parts, chloroprene rubber is 6-14 parts, polyethylene terephthalate is 7-15 parts, polyvinyl alcohol is 4-13 parts, polyisobutylene is 54-64 parts, and polycarbonate is 4-13 parts.

[0010] Preferably, the base material comprises 20-30 parts of EPDM rubber, 5-13 parts of chloroprene rubber, 8-14 parts of polyethylene terephthalate, 5-12 parts of polyvinyl alcohol, 55-63 parts of polyisobutylene and 5-12 parts of polycarbonate.

[0011] Preferably, the EPDM base material is 21-29 parts, chloroprene rubber is 6-12 parts, polyethylene terephthalate is 9-13 parts, polyvinyl alcohol is 6-11 parts, polyisobutylene is 56-62 parts, and polycarbonate is 6-11 parts.

[0012] Preferably, the base material comprises 22-28 parts of EPDM rubber, 7-11 parts of chloroprene rubber, 8-12 parts of polyethylene terephthalate, 7-10 parts of polyvinyl alcohol, 57-61 parts of polyisobutylene and 7-12 parts of polycarbonate.

[0013] Preferably, the base material comprises 23-27 parts of EPDM rubber, 8-10 parts of chloroprene rubber, 9-11 parts of polyethylene terephthalate, 8-9 parts of polyvinyl alcohol, 58-60 parts of polyisobutylene and 8-11 parts of polycarbonate.

[0014] Preferably, 24 parts of EPDM rubber base material, 9 parts of chloroprene rubber, 10 parts of polyethylene terephthalate, 7 parts of polyvinyl alcohol, 59 parts of polyisobutylene, and 9 parts of polycarbonate.

[0015] Preferably, the method comprises the following preparation steps:

[0016] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0017] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0018] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. By adding polycarbonate to the mixed particles, the rubber can still maintain a strong antistatic function at high temperatures. At the same time, the added chloroprene rubber and polyisobutylene can improve the mechanical properties of the rubber while improving the acid, alkali and salt corrosion resistance of the rubber, greatly extending the service life of the rubber;

[0021] 2. By adding polyethylene terephthalate into the mixed particles, the rubber can still maintain a strong antistatic function at a high temperature of 120°C, thereby enhancing the electrical properties of the EPDM rubber compound. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The present invention provides a technical solution:

[0024] Embodiment 1: An EPDM rubber compound: comprising the following components counted by weight: 18-32 parts of EPDM rubber base material, 5-15 parts of chloroprene rubber, 6-16 parts of polyethylene terephthalate, 3-14 parts of polyvinyl alcohol, 54-65 parts of polyisobutylene, and 3-14 parts of polycarbonate.

[0025] Preparation steps:

[0026] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0027] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0028] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0029] Embodiment 2: An EPDM rubber compound: comprising the following components counted by weight: 19-31 parts of EPDM rubber base material, 6-14 parts of chloroprene rubber, 7-15 parts of polyethylene terephthalate, 4-13 parts of polyvinyl alcohol, 54-64 parts of polyisobutylene, and 4-13 parts of polycarbonate.

[0030] Preparation steps:

[0031] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0032] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0033] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0034] Embodiment 3: An EPDM rubber compound: comprising the following components counted by weight: 20-30 parts of EPDM rubber base material, 5-13 parts of chloroprene rubber, 8-14 parts of polyethylene terephthalate, 5-12 parts of polyvinyl alcohol, 55-63 parts of polyisobutylene, and 5-12 parts of polycarbonate.

[0035] Preparation steps:

[0036] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0037] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0038] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0039] Embodiment 4: An EPDM rubber compound comprises the following components counted by weight: 21-29 parts of EPDM rubber base material, 6-12 parts of chloroprene rubber, 9-13 parts of polyethylene terephthalate, 6-11 parts of polyvinyl alcohol, 56-62 parts of polyisobutylene, and 6-11 parts of polycarbonate.

[0040] Preparation steps:

[0041] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0042] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0043] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0044] Embodiment 5: An EPDM rubber compound comprises the following components counted by weight: 22-28 parts of EPDM rubber base material, 7-11 parts of chloroprene rubber, 8-12 parts of polyethylene terephthalate, 7-10 parts of polyvinyl alcohol, 57-61 parts of polyisobutylene, and 7-12 parts of polycarbonate.

[0045] Preparation steps:

[0046] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0047] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0048] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0049] Example 6: An EPDM rubber compound comprises the following components counted by weight: 23-27 parts of EPDM rubber base material, 8-10 parts of chloroprene rubber, 9-11 parts of polyethylene terephthalate, 8-9 parts of polyvinyl alcohol, 58-60 parts of polyisobutylene, and 8-11 parts of polycarbonate.

[0050] Preparation steps:

[0051] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0052] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0053] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0054] Example 7: An EPDM rubber compound comprises the following components counted by weight: 24 parts of EPDM rubber base material, 9 parts of chloroprene rubber, 10 parts of polyethylene terephthalate, 7 parts of polyvinyl alcohol, 59 parts of polyisobutylene, and 9 parts of polycarbonate.

[0055] Preparation steps:

[0056] S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process;

[0057] S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing;

[0058] S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

[0059] Performance Test:

[0060] The finished products obtained in Examples 1-6 of the present invention were compared with the finished product obtained in Example 7 for performance testing.

[0061] Table 1 is the performance test data:

[0062] Tensile strength(Mpa) Surface impedance(ohm) Molecular viscosity (cP) Example 1 120 10+2ohm 9100cP Example 2 118 10+4ohm 9050cP Example 3 120 10+6ohm 9070cP Example 4 118 10+70hm 9090cP Example 5 117 10+9ohm 9050cP Example 6 118 10+8ohm 9070cP Example 7 121 10+70hm 9150cP

[0063] Based on the above data, it can be seen that the present invention has excellent performance in maintaining stable molecular viscosity, anti-stretching and anti-static fields at high temperatures. Based on the data, it can be seen that Example 5 is the best in maintaining stable molecular viscosity, anti-stretching and anti-static fields at high temperatures.

[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An EPDM rubber compound, characterized in that: The invention comprises the following components counted in parts by weight: 18-32 parts of EPDM rubber base material, 5-15 parts of chloroprene rubber, 6-16 parts of polyethylene terephthalate, 3-14 parts of polyvinyl alcohol, 54-65 parts of polyisobutylene and 3-14 parts of polycarbonate.

2. An EPDM rubber compound according to claim 1, characterized in that: The invention comprises the following components counted in parts by weight: 19-31 parts of EPDM rubber base material, 6-14 parts of chloroprene rubber, 7-15 parts of polyethylene terephthalate, 4-13 parts of polyvinyl alcohol, 54-64 parts of polyisobutylene and 4-13 parts of polycarbonate.

3. The EPDM rubber compound according to claim 1, characterized in that: The invention comprises the following components counted by weight: 20-30 parts of EPDM rubber base material, 5-13 parts of chloroprene rubber, 8-14 parts of polyethylene terephthalate, 5-12 parts of polyvinyl alcohol, 55-63 parts of polyisobutylene and 5-12 parts of polycarbonate.

4. The EPDM rubber compound according to claim 1, characterized in that: The invention comprises the following components counted by weight: 21-29 parts of EPDM rubber base material, 6-12 parts of chloroprene rubber, 9-13 parts of polyethylene terephthalate, 6-11 parts of polyvinyl alcohol, 56-62 parts of polyisobutylene and 6-11 parts of polycarbonate.

5. The EPDM rubber compound according to claim 1, characterized in that: The invention comprises the following components counted by weight: 22-28 parts of EPDM rubber base material, 7-11 parts of chloroprene rubber, 8-12 parts of polyethylene terephthalate, 7-10 parts of polyvinyl alcohol, 57-61 parts of polyisobutylene and 7-12 parts of polycarbonate.

6. The EPDM rubber compound according to claim 1, characterized in that: The invention comprises the following components counted by weight: 23-27 parts of EPDM rubber base material, 8-10 parts of chloroprene rubber, 9-11 parts of polyethylene terephthalate, 8-9 parts of polyvinyl alcohol, 58-60 parts of polyisobutylene and 8-11 parts of polycarbonate.

7. The EPDM rubber compound according to claim 1, characterized in that: The invention comprises the following components counted in parts by weight: 24 parts of EPDM rubber base material, 9 parts of chloroprene rubber, 10 parts of polyethylene terephthalate, 7 parts of polyvinyl alcohol, 59 parts of polyisobutylene and 9 parts of polycarbonate.

8. The EPDM rubber compound according to claim 1, characterized in that: The method comprises the following preparation steps: S1: Put EPDM rubber base material, chloroprene rubber and polyisobutylene raw materials into the same container in turn, mix the materials into a qualified uniform ratio, put small particles of the mixed material into a mixing chamber, mix the mixture in a certain proportion, and then further crush the particles of the mixture to make the particles of the mixture smaller, which is helpful for the full fusion of the mixture during the mixing process; S2: then raising the temperature in the stirring chamber to 115°C-135°C, adding polyvinyl alcohol, polycarbonate and polyethylene terephthalate, and then continuing the mixing step in the stirring chamber. When the mixing step is completed, the stirring chamber is cooled to 95°C-98°C and polyethylene terephthalate is added for secondary mixing; S3: After all the raw materials are mixed, the processed mixture is transferred to a foaming furnace for foaming and condensation, the foamed rubber is loaded into a molding mold, and finally the molded rubber product is placed on a 140°C heating rack for baking to form a solid product, thereby completing the production of EPDM rubber compound.

Citation Information

Patent Citations

  • Filter adhesive film prepared by mixing neoprene and ethylene propylene diene monomer (EPDM)

    CN102952478A