High-strength hot box resin and preparation method thereof
By using sugarcane bagasse extract and composite heat stabilizer in hot core box resin, the problems of insufficient strength and environmental protection of existing resins are solved, high strength, good heat conduction and thermal stability are achieved, and the production efficiency of the foundry industry is improved. and environmental protection.
Patent Information
- Application Number
- CN202411058222.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing hot core box resin has poor strength, environmental protection, thermal stability and thermal conductivity, making it difficult to meet the needs of modern industry for high-strength adhesives.
Using a combination of phenolic compounds, bagasse extract, sodium hydroxide solution, composite heat stabilizer and coupling agent, part of the phenol is replaced by bagasse extract, and the composite heat stabilizer is used to improve the thermal conductivity and environmental protection of the resin, and The cohesion and mechanical strength of the resin are enhanced through silicon-oxygen bonds.
Significantly improves the strength, thermal conductivity and thermal stability of the thermal core box resin, reduces environmental pollution risks and production costs, and extends the service life of the resin.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hot box resin preparation, and in particular relates to a high-strength hot box resin and a preparation method thereof. Background Art
[0002] With the development of modern industry, especially the progress of foundry industry, the performance requirements of resin binders are constantly increasing. As a binder that cures under heating conditions, hot box resin plays a key role in the core making process of mass production. Therefore, in order to meet the market demand for higher strength and higher performance binders, the research on high-strength hot box resin has become particularly important.
[0003] Secondly, high-strength hot-box resin has a series of significant advantages, such as high strength, fast curing, high production efficiency, low viscosity, easy sand mixing, good core sand fluidity, good moisture resistance, long sand core storage time, etc. These characteristics make high-strength hot-box resin widely used in the production of cast steel, cast iron and non-ferrous alloy castings. By continuously optimizing the performance of resin, the quality of castings can be further improved, production costs can be reduced, production efficiency can be improved, and the progress of the entire foundry industry can be promoted.
[0004] Patent CN 104193936 B discloses a hot box resin for casting and a preparation method thereof. The raw materials and mass percentages thereof are: 90-95% furfuryl alcohol, 0.2-1.0% solid formaldehyde, 1.0-2.0% urea, 2.0-5.0% monohydric alcohol and 0.2-1% coupling agent. The preparation process uses solid formaldehyde instead of liquid formaldehyde, which reduces the dehydration link in the preparation process, achieving the purpose of environmental protection, energy saving and efficiency improvement; the prepared hot box resin has the characteristics of low free formaldehyde content, high strength and low viscosity, but the strength, environmental protection, thermal stability and thermal conductivity of the hot box resin prepared by the method still have room for improvement. Summary of the invention
[0005] The object of the present invention is to provide a high-strength hot box resin and a preparation method thereof, so as to solve the technical problems of poor strength, environmental protection, thermal stability and thermal conductivity of the hot box resin in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions: The invention provides a high-strength hot box resin, which is composed of the following components in parts by weight: 14-19 parts of phenolic compounds, 20-25 parts of aldehyde compounds, 6-12 parts of bagasse extracts, 2-4 parts of sodium hydroxide solutions, 2-5 parts of composite heat stabilizers, and 1-4 parts of coupling agents, wherein the bagasse extract is extracted from the bagasse using a hydrochloric acid methanol solution, and the composite heat stabilizer is prepared from polyetheretherketone and silicone gel.
[0007] Preferably, the method for preparing the bagasse extract comprises the following steps: Q1: The collected bagasse is crushed, sieved, and subjected to reflux extraction treatment with a mixed solution of benzene and ethanol. After the treatment, the bagasse is placed in a fume hood and vacuum dried to obtain a crude bagasse product; Q2: Place the crude sugarcane bagasse in a ball mill for grinding, place the ground crude sugarcane bagasse in a container, add hydrochloric acid methanol solution, seal, stir, centrifuge, wash and centrifuge, collect the supernatant, evaporate and concentrate, and freeze-dry to obtain the sugarcane bagasse extract.
[0008] In the above process, the bagasse is treated with a mixed solution of benzene and ethanol to remove organic matter such as fatty acids and resins, and then the crude bagasse is separated and extracted by ball milling. Finally, hydrochloric acid methanol solution is used for extraction to obtain the bagasse extract.
[0009] Preferably, in Q1, the sieve size is 60-80 mesh, the solid content of bagasse is ≥98%, the dosage ratio of bagasse, benzene and ethanol is (100-200) g: (1.8-2.2) L: 1 L, the reflux extraction treatment time is 24-28 h, the placement time in the fume hood is 12-15 h, the vacuum drying temperature is 40-50 ° C, and the time is 20-28 h.
[0010] Preferably, in Q2, the rotation speed of the ball mill is 400-600 rpm, the grinding time is 22-26 h, the usage ratio of the ground crude bagasse and the hydrochloric acid methanol solution is (6-8) g: (150-200) mL, the concentration of the hydrochloric acid methanol solution is 1.36 mol / L, the stirring temperature is 25-32°C, the stirring time is 24-26 h, the centrifugal speed is 4000-6000 rpm, the temperature is 3-5°C, the time is 20-25 min, the washing and centrifugation are carried out with anhydrous methanol, the operation is repeated 3-5 times, and the freeze-drying temperature is -80 to -90°C for 24-30 h.
[0011] Preferably, the preparation method of the composite thermal stabilizer comprises the following steps: S1: Methyl vinyl silicone rubber and vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) are mixed to obtain a vinyl compound, which is then mixed with hydrogen-containing silicone oil, polymethyl hydrogen siloxane, a platinum catalyst and an inhibitor, and then placed in a vacuum mixer for mixing to obtain a silicone mixture; S2: mixing spherical aluminum oxide and zinc oxide to obtain a mixed filler, placing the mixed filler and the organic silicon mixture in a vacuum mixer to mix them to obtain an organic silicon gel; S3: After heating and melting diphenyl sulfone, 4,4-difluorobenzophenone, hydroquinone and sodium carbonate are added under the protection of helium, and after heating treatment, cooling and purification are performed to obtain composite polyetheretherketone; S4: Add the composite polyetheretherketone into a container containing cyclopentane sulfone, heat and stir under helium protection, then slowly add the silicone gel into the container, stir after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry to obtain a composite thermal stabilizer.
[0012] In the above process, silicone oils with different viscosities were used as the matrix, and aluminum oxide and zinc oxide were used as fillers to prepare organic silicone gel. Subsequently, 4,4-difluorobenzophenone and hydroquinone were used in the presence of diphenyl sulfone and sodium carbonate as solvents and catalysts to prepare composite polyetheretherketone. The organic silicone gel and the composite polyetheretherketone were compounded to obtain a composite thermal stabilizer. The reaction process of the composite polyetheretherketone is as follows:
[0013] Preferably, in S1, the viscosity of the methyl vinyl silicone rubber is 500 Pa·s, the viscosity of the vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) is 8000 Pa·s, the mass ratio of the methyl vinyl silicone rubber to the vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) is 2:(8-10), and the mass ratio of the vinyl complex, hydrogen-containing silicone oil, polymethyl hydrogen siloxane, platinum catalyst and inhibitor is (100-120):(5-6):(2. 5-2.8): (0.8-1): (0.3-0.35), the mixing speed is 500-600rpm, and the mixing time is 3-5min; in S2, the spherical diameter of spherical alumina is 2μm, the particle size of zinc oxide is 300nm, the mass ratio of alumina to zinc oxide is 2: (0.8-1.2), the mass ratio of the mixed filler to the silicone mixture is 1: (8-10), the speed of the vacuum mixer is 500-600rpm, and the mixing time is 5-10min.
[0014] Preferably, in S3, the heating melting temperature is 140-150°C, the mass ratio of diphenyl sulfone, 4,4-difluorobenzophenone, hydroquinone and sodium carbonate is (163.8-282.1): (140.47-184.29): (71.10-93.32): (82.56-108.24), and the heating treatment process is: heating at 190°C, 220°C, 250°C and 280°C for 40 min, and finally heated at 310°C for 30 min, and purified with acetone and water using a Soxhlet extractor; in the S4, the mass ratio of the composite polyetheretherketone, cyclopentane sulfone, and silicone gel is (10-12): (32-38): (8-10), the heating temperature is 280-300°C, the stirring time is 3-5h, the stirring time after uniform dispersion is 2-4h, and the vacuum drying temperature is 80-90°C and the time is 6-8h.
[0015] Preferably, the method for preparing the high-strength hot box resin comprises the following steps: Step (1): adding a phenolic compound, a bagasse extract and a sodium hydroxide solution into a container, placing a rotor, and then adding an aldehyde compound, heating the container to react, and obtaining a prepolymer product; In the above process, bagasse extract is used to replace part of phenolic compounds to synthesize phenolic resin, which improves the environmental protection of the resin and reduces the release of aldehyde compounds during use.
[0016] Step (2): The prepolymer product, the composite thermal stabilizer and the coupling agent are mixed and stirred, reacted at a constant temperature, and distilled under reduced pressure to obtain a high-strength hot core box resin.
[0017] Preferably, in step (1), the volume concentration of the sodium hydroxide solution is 15vt%, the heating temperature is 70-100°C, and the reaction time is 1-3h.
[0018] Preferably, in step (2), the mixing and stirring time is 1-2 h, the constant temperature reaction temperature is 60-70° C., and the reaction time is 1.5-3 h.
[0019] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. The present invention first extracts bagasse extract from solid waste bagasse, and uses the bagasse extract to replace part of phenol to reduce the release of formaldehyde in the preparation process of hot box resin, thereby increasing the environmental protection of the resin. Subsequently, silicone oil with different viscosities is used as a matrix and aluminum oxide and zinc oxide are used as fillers to prepare silicone gel. Then, 4,4-difluorobenzophenone and hydroquinone are used as raw materials to synthesize a composite polyetheretherketone with excellent strength, which is compounded with the silicone gel to prepare a composite thermal stabilizer. The hot box resin prepared by the method has excellent strength, thermal conductivity, thermal stability and environmental protection.
[0020] 2. The present invention uses bagasse extract to replace part of phenol, which can not only improve the environmental friendliness of the hot box resin, but also improve the thermal stability. The active groups (such as hydroxyl, methoxy, etc.) in the bagasse extract can react with formaldehyde, reducing the demand for formaldehyde in the synthesis process and reducing the environmental risk of the resin. The addition of bagasse extract can also improve the curing process of the resin, reduce the emission of volatile organic matter in the curing process, and reduce environmental pollution in the production process. At the same time, the high thermal stability of the bagasse extract enables the hot box resin to maintain good performance in a high temperature environment, extend its service life, reduce the replacement frequency, and reduce the pressure on the environment.
[0021] 3. The present invention uses methyl vinyl silicone rubber, vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), hydrogen-containing silicone oil and polymethyl hydrogen siloxane as raw materials, aluminum oxide and zinc oxide as fillers to synthesize an organic silicon mixture, and then uses 4,4-difluorobenzophenone and hydroquinone as raw materials to synthesize a composite polyetheretherketone, and combines the two to obtain a composite thermal stabilizer. The silicon-oxygen bond in the silicone mixture has a high bond energy and can remain stable under high temperature conditions, so that the composite heat stabilizer also has excellent thermal stability. The flexibility of the silicon-oxygen chain segment and the low intermolecular friction of the silicone material itself also contribute to the transfer of heat energy. When it is added to the hot box resin as part of the composite heat stabilizer, the thermal conductivity of the overall hot box resin can be improved. The molecular chain of the composite polyetheretherketone contains a large number of aromatic rings and polar groups, which gives it excellent thermal stability and strength. The added inhibitor can effectively inhibit the side reactions in the hydrosilylation reaction, reduce unnecessary heat generation, and further improve the thermal stability of the hot box resin. Aluminum oxide and zinc oxide as fillers are evenly dispersed in the resin to form an effective reinforcement network, so that the resin can better resist deformation and damage when subjected to external forces. At the same time, the silicon-oxygen bonds in the silicone mixture can react with the hydroxyl or carboxyl groups in the resin to form chemical bonds, enhance the cohesion and mechanical strength of the resin, and thus increase the strength of the hot box resin. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0023] This embodiment discloses a method for preparing a bagasse extract, comprising the following steps: Q1: 150 g of collected bagasse (solid content ≥ 98%) was crushed, passed through an 80-mesh sieve, and subjected to reflux extraction treatment with a mixed solution of 2 L benzene and 1 L ethanol. After 24 h of treatment, the bagasse was placed in a fume hood for 15 h and vacuum dried at 50 ° C for 28 h to obtain a crude bagasse product; Q2: The crude sugarcane bagasse was placed in a ball mill for grinding at 600 rpm for 24 h. 7 g of the ground crude sugarcane bagasse was placed in a container, 150 mL of 1.36 mol / L hydrochloric acid methanol solution was added and sealed. The container was stirred at 32 ° C for 24 h, centrifuged at 6000 rpm and 5 ° C for 25 min, washed and centrifuged with anhydrous methanol, and the operation was repeated 3 times. The supernatant was collected, evaporated and concentrated, and freeze-dried at -80 ° C for 24 h to obtain the sugarcane bagasse extract.
[0024] This embodiment discloses a method for preparing a composite thermal stabilizer, comprising the following steps: S1: 20 g of methyl vinyl silicone rubber with a viscosity of 500 Pa·s and 90 g of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) with a viscosity of 8000 Pa·s were mixed to obtain a vinyl compound, 110 g of the vinyl compound was mixed with 5.5 g of hydrogen-containing silicone oil, 2.65 g of polymethyl hydrogen siloxane, 0.9 g of platinum catalyst and 0.32 g of triethylamine, and then placed in a vacuum mixer at 600 rpm for 5 min to obtain a silicone mixture; S2: 2 g of spherical aluminum oxide with a particle size of 2 μm and 1 g of zinc oxide with a spherical diameter of 300 nm were mixed to obtain a mixed filler, and 1 g of the mixed filler and 9 g of the organic silicon mixture were placed in a vacuum mixer at 500 rpm and mixed for 10 min to obtain an organic silicon gel; S3: After heating 216.13g of diphenyl sulfone at 150°C to melt, under the protection of helium, 163.65g of 4,4-difluorobenzophenone, 82.58g of hydroquinone and 95.39g of sodium carbonate were added, and the temperature was increased. The process was: heating at 190°C, 220°C, 250°C and 280°C for 40min respectively, and finally heating at 310°C for 30min. After the temperature increase treatment, cooling was performed, and purification was performed with acetone and water using a Soxhlet extractor to obtain a composite polyetheretherketone; S4: Add 11g of composite polyetheretherketone into a container containing 34g of cyclopentane sulfone, heat to 280°C under helium protection and stir for 4h, then slowly add 9g of silicone gel into the container, stir for 4h after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry at 80°C for 6h to obtain a composite thermal stabilizer.
[0025] The present embodiment discloses a high-strength hot box resin, which is composed of the following components in parts by weight: 16.5 parts of phenol, 22.5 parts of formaldehyde solution, 9 parts of bagasse extract, 3 parts of sodium hydroxide solution, 3.5 parts of composite heat stabilizer, and 2.5 parts of silane coupling agent KH-550.
[0026] This embodiment discloses a method for preparing a high-strength hot box resin, comprising the following steps: Step (1): adding phenol, bagasse extract and a sodium hydroxide solution with a volume concentration of 15 vt% into a container, placing a rotor, and then adding a formaldehyde solution with a volume fraction of 40 vt%, heating to 80° C. for reaction for 3 hours to obtain a prepolymer product; Step (2): The prepolymer product, the composite thermal stabilizer and the silane coupling agent KH-550 are mixed and stirred for 2 hours, reacted at a constant temperature of 70° C. for 2 hours, and distilled under reduced pressure to obtain a high-strength hot core box resin. Example 2
[0027] This embodiment discloses a method for preparing a bagasse extract, comprising the following steps: Q1: 100g of collected bagasse (solid content ≥ 98%) was crushed, passed through an 80-mesh sieve, and subjected to reflux extraction treatment with a mixed solution of 1.8L benzene and 1L ethanol. After 24h of treatment, the bagasse was placed in a fume hood for 15h and vacuum dried at 50℃ for 28h to obtain a crude bagasse; Q2: The crude sugarcane bagasse was placed in a ball mill for grinding at 600 rpm for 24 h. 6 g of the ground crude sugarcane bagasse was placed in a container, 200 mL of 1.36 mol / L hydrochloric acid methanol solution was added and sealed. The container was stirred at 32 ° C for 24 h, centrifuged at 6000 rpm and 5 ° C for 25 min, washed and centrifuged with anhydrous methanol, and the operation was repeated 3 times. The supernatant was collected, evaporated and concentrated, and freeze-dried at -80 ° C for 24 h to obtain the sugarcane bagasse extract.
[0028] This embodiment discloses a method for preparing a composite thermal stabilizer, comprising the following steps: S1: 20 g of methyl vinyl silicone rubber with a viscosity of 500 Pa·s and 80 g of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) with a viscosity of 8000 Pa·s were mixed to obtain a vinyl compound, 100 g of the vinyl compound was mixed with 5 g of hydrogenated silicone oil, 2.6 g of polymethyl hydrogen siloxane, 0.95 g of platinum catalyst and 0.35 g of triethylamine, and then placed in a vacuum mixer at 600 rpm for 5 min to obtain a silicone mixture; S2: 2 g of spherical aluminum oxide with a particle size of 2 μm and 0.8 g of zinc oxide with a spherical diameter of 300 nm were mixed to obtain a mixed filler, and 1 g of the mixed filler and 8 g of the organic silicon mixture were placed in a vacuum mixer at 500 rpm and mixed for 10 min to obtain an organic silicon gel; S3: After heating 165.71g of diphenyl sulfone at 150°C to melt, under the protection of helium, 142.74g of 4,4-difluorobenzophenone, 72.23g of hydroquinone and 84.67g of sodium carbonate were added, and the temperature was increased. The process was: heating at 190°C, 220°C, 250°C and 280°C for 40min respectively, and finally heating at 310°C for 30min. After the temperature increase treatment, cooling was performed, and purification was performed with acetone and water using a Soxhlet extractor to obtain a composite polyetheretherketone; S4: Add 10g of composite polyetheretherketone into a container containing 32g of cyclopentane sulfone, heat to 280°C under helium protection and stir for 4h, then slowly add 8g of silicone gel into the container, stir for 4h after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry at 80°C for 6h to obtain a composite thermal stabilizer.
[0029] The present embodiment discloses a high-strength hot box resin, which is composed of the following components in parts by weight: 14 parts of phenol, 20 parts of formaldehyde solution, 6 parts of bagasse extract, 2 parts of sodium hydroxide solution, 2 parts of composite heat stabilizer, and 1 part of silane coupling agent KH-550.
[0030] This embodiment discloses a method for preparing a high-strength hot box resin, comprising the following steps: Step (1): adding phenol, bagasse extract and a sodium hydroxide solution with a volume concentration of 15 vt% into a container, placing a rotor, and then adding a formaldehyde solution with a volume fraction of 40 vt%, heating to 80° C. for reaction for 3 hours to obtain a prepolymer product; Step (2): The prepolymer product, the composite thermal stabilizer and the silane coupling agent KH-550 are mixed and stirred for 2 hours, reacted at a constant temperature of 70° C. for 2 hours, and distilled under reduced pressure to obtain a high-strength hot core box resin. Example 3
[0031] This embodiment discloses a method for preparing a bagasse extract, comprising the following steps: Q1: 200 g of collected bagasse (solid content ≥ 98%) was crushed, passed through an 80-mesh sieve, and subjected to reflux extraction treatment with a mixed solution of 2.2 L benzene and 1 L ethanol. After 24 h of treatment, the bagasse was placed in a fume hood for 15 h and vacuum dried at 50 ° C for 28 h to obtain a crude bagasse; Q2: The crude sugarcane bagasse was placed in a ball mill for grinding at 600 rpm for 24 h. 8 g of the ground crude sugarcane bagasse was placed in a container, 175 mL of 1.36 mol / L hydrochloric acid methanol solution was added and sealed. The container was stirred at 32 ° C for 24 h, centrifuged at 6000 rpm and 5 ° C for 25 min, washed and centrifuged with anhydrous methanol, and the operation was repeated 3 times. The supernatant was collected, evaporated and concentrated, and freeze-dried at -80 ° C for 24 h to obtain the sugarcane bagasse extract.
[0032] This embodiment discloses a method for preparing a composite thermal stabilizer, comprising the following steps: S1: 20 g of methyl vinyl silicone rubber with a viscosity of 500 Pa·s and 100 g of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) with a viscosity of 8000 Pa·s were mixed to obtain a vinyl compound, 120 g of the vinyl compound was mixed with 6 g of hydrogen-containing silicone oil, 2.5 g of polymethyl hydrogen siloxane, 0.97 g of platinum catalyst and 0.3 g of triethylamine, and then placed in a vacuum mixer at 600 rpm for 5 min to obtain a silicone mixture; S2: 2 g of spherical aluminum oxide with a particle size of 2 μm and 1.2 g of zinc oxide with a spherical diameter of 300 nm were mixed to obtain a mixed filler, and 1 g of the mixed filler and 10 g of the organic silicon mixture were placed in a vacuum mixer at 500 rpm and mixed for 10 min to obtain an organic silicon gel; S3: After heating 279.85g of diphenyl sulfone at 150°C to melt, under the protection of helium, 182.93g of 4,4-difluorobenzophenone, 92.35g of hydroquinone and 106.42g of sodium carbonate were added, and the temperature was increased. The process was: heating at 190°C, 220°C, 250°C and 280°C for 40min respectively, and finally heating at 310°C for 30min. After the temperature treatment, cooling was performed, and purification was performed with acetone and water using a Soxhlet extractor to obtain a composite polyetheretherketone; S4: Add 12g of composite polyetheretherketone into a container containing 38g of cyclopentane sulfone, heat to 280°C under helium protection and stir for 4h, then slowly add 10g of silicone gel into the container, stir for 4h after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry at 80°C for 6h to obtain a composite thermal stabilizer.
[0033] The present embodiment discloses a high-strength hot core box resin, which is composed of the following components in parts by weight: 19 parts of phenol, 25 parts of formaldehyde solution, 12 parts of bagasse extract, 4 parts of sodium hydroxide solution, 5 parts of composite heat stabilizer, and 4 parts of silane coupling agent KH-550.
[0034] This embodiment discloses a method for preparing a high-strength hot box resin, comprising the following steps: Step (1): adding phenol, bagasse extract and a sodium hydroxide solution with a volume concentration of 15 vt% into a container, placing a rotor, and then adding a formaldehyde solution with a volume fraction of 40 vt%, heating to 80° C. for reaction for 3 hours to obtain a prepolymer product; Step (2): The prepolymer product, the composite thermal stabilizer and the silane coupling agent KH-550 are mixed and stirred for 2 hours, reacted at a constant temperature of 70° C. for 2 hours, and distilled under reduced pressure to obtain a high-strength hot core box resin. Example 4
[0035] This embodiment discloses a method for preparing a bagasse extract, comprising the following steps: Q1: 120 g of collected bagasse (solid content ≥ 98%) was crushed, passed through an 80-mesh sieve, and subjected to reflux extraction treatment with a mixed solution of 1.9 L benzene and 1 L ethanol. After 24 h of treatment, the bagasse was placed in a fume hood for 15 h and vacuum dried at 50 ° C for 28 h to obtain a crude bagasse product; Q2: The crude sugarcane bagasse was placed in a ball mill for grinding at 600 rpm for 24 h. 6.5 g of the ground crude sugarcane bagasse was placed in a container, 180 mL of 1.36 mol / L hydrochloric acid methanol solution was added and sealed. The mixture was stirred at 32 °C for 24 h, centrifuged at 6000 rpm and 5 °C for 25 min, washed and centrifuged with anhydrous methanol, and the operation was repeated 3 times. The supernatant was collected, evaporated and concentrated, and freeze-dried at -80 °C for 24 h to obtain the sugarcane bagasse extract.
[0036] This embodiment discloses a method for preparing a composite thermal stabilizer, comprising the following steps: S1: 20 g of methyl vinyl silicone rubber with a viscosity of 500 Pa·s and 85 g of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) with a viscosity of 8000 Pa·s were mixed to obtain a vinyl compound, 105 g of the vinyl compound was mixed with 5.2 g of hydrogen-containing silicone oil, 2.8 g of polymethyl hydrogen siloxane, 0.8 g of platinum catalyst and 0.33 g of triethylamine, and then placed in a vacuum mixer at 600 rpm for 5 min to obtain a silicone mixture; S2: 2 g of spherical aluminum oxide with a particle size of 2 μm and 0.9 g of zinc oxide with a spherical diameter of 300 nm were mixed to obtain a mixed filler, and 1 g of the mixed filler and 8.5 g of the organic silicon mixture were mixed in a vacuum mixer at 500 rpm for 10 min to obtain an organic silicon gel; S3: After heating 243.24g of diphenyl sulfone at 150°C to melt, under the protection of helium, 151.56g of 4,4-difluorobenzophenone, 85.91g of hydroquinone and 88.71g of sodium carbonate were added, and the temperature was increased. The process was: heating at 190°C, 220°C, 250°C and 280°C for 40min respectively, and finally heating at 310°C for 30min. After the temperature increase treatment, cooling was performed, and purification was performed with acetone and water using a Soxhlet extractor to obtain a composite polyetheretherketone; S4: Add 10.5g of composite polyetheretherketone into a container containing 36g of cyclobutane sulfone, heat to 280°C under helium protection and stir for 4h, then slowly add 8.5g of silicone gel into the container, stir for 4h after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry at 80°C for 6h to obtain a composite thermal stabilizer.
[0037] The present embodiment discloses a high-strength hot core box resin, which is composed of the following components in parts by weight: 15 parts of phenol, 22 parts of formaldehyde solution, 8 parts of bagasse extract, 2.5 parts of sodium hydroxide solution, 3 parts of composite heat stabilizer, and 2 parts of silane coupling agent KH-550.
[0038] This embodiment discloses a method for preparing a high-strength hot box resin, comprising the following steps: Step (1): adding phenol, bagasse extract and a sodium hydroxide solution with a volume concentration of 15 vt% into a container, placing a rotor, and then adding a formaldehyde solution with a volume fraction of 40 vt%, heating to 80° C. for reaction for 3 hours to obtain a prepolymer product; Step (2): The prepolymer product, the composite thermal stabilizer and the silane coupling agent KH-550 are mixed and stirred for 2 hours, reacted at a constant temperature of 70° C. for 2 hours, and distilled under reduced pressure to obtain a high-strength hot core box resin. Example 5
[0039] This embodiment discloses a method for preparing a bagasse extract, comprising the following steps: Q1: 180 g of collected bagasse (solid content ≥ 98%) was crushed, passed through an 80-mesh sieve, and subjected to reflux extraction treatment with a mixed solution of 2.1 L benzene and 1 L ethanol. After 24 h of treatment, the bagasse was placed in a fume hood for 15 h and vacuum dried at 50 ° C for 28 h to obtain a crude bagasse; Q2: The crude sugarcane bagasse was placed in a ball mill for grinding at 600 rpm for 24 h. 7.5 g of the ground crude sugarcane bagasse was placed in a container, 160 mL of 1.36 mol / L hydrochloric acid methanol solution was added and sealed, stirred at 32 ° C for 24 h, centrifuged at 6000 rpm and 5 ° C for 25 min, washed and centrifuged with anhydrous methanol, repeated the operation 3 times, collected the supernatant, evaporated and concentrated, and freeze-dried at -80 ° C for 24 h to obtain the sugarcane bagasse extract.
[0040] This embodiment discloses a method for preparing a composite thermal stabilizer, comprising the following steps: S1: 20 g of methyl vinyl silicone rubber with a viscosity of 500 Pa·s and 95 g of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) with a viscosity of 8000 Pa·s were mixed to obtain a vinyl compound, 115 g of the vinyl compound was mixed with 5.7 g of hydrogen-containing silicone oil, 2.7 g of polymethyl hydrogen siloxane, 1 g of platinum catalyst and 0.31 g of triethylamine, and then placed in a vacuum mixer at 600 rpm for 5 min to obtain a silicone mixture; S2: 2 g of spherical aluminum oxide with a particle size of 2 μm and 1.1 g of zinc oxide with a spherical diameter of 300 nm were mixed to obtain a mixed filler, and 1 g of the mixed filler and 9.5 g of the organic silicon mixture were placed in a vacuum mixer at 500 rpm and mixed for 10 min to obtain an organic silicon gel; S3: After heating 180.58g of diphenyl sulfone at 150°C to melt, under the protection of helium, 177.89g of 4,4-difluorobenzophenone, 75.47g of hydroquinone and 99.15g of sodium carbonate were added, and the temperature was increased. The process was: heating at 190°C, 220°C, 250°C and 280°C for 40min respectively, and finally heating at 310°C for 30min. After the temperature increase treatment, cooling was performed, and purification was performed with acetone and water using a Soxhlet extractor to obtain a composite polyetheretherketone; S4: Add 11.5g of composite polyetheretherketone into a container containing 35g of cyclopentane sulfone, heat to 280°C under helium protection and stir for 4h, then slowly add 9.5g of silicone gel into the container, stir for 4h after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry at 80°C for 6h to obtain a composite thermal stabilizer.
[0041] The present embodiment discloses a high-strength hot box resin, which is composed of the following components in parts by weight: 18 parts of phenol, 23 parts of formaldehyde solution, 11 parts of bagasse extract, 3.5 parts of sodium hydroxide solution, 4 parts of composite heat stabilizer, and 3 parts of silane coupling agent KH-550.
[0042] This embodiment discloses a method for preparing a high-strength hot box resin, comprising the following steps: Step (1): adding phenol, bagasse extract and a sodium hydroxide solution with a volume concentration of 15 vt% into a container, placing a rotor, and then adding a formaldehyde solution with a volume fraction of 40 vt%, heating to 80° C. for reaction for 3 hours to obtain a prepolymer product; Step (2): The prepolymer product, the composite thermal stabilizer and the silane coupling agent KH-550 are mixed and stirred for 2 hours, reacted at a constant temperature of 70° C. for 2 hours, and distilled under reduced pressure to obtain a high-strength hot core box resin.
[0043] Comparative Example 1 Comparative Example 1 Compared with Example 1, in the process of preparing the bagasse extract in Comparative Example 1, no hydrochloric acid methanol solution was added, and other conditions remained unchanged.
[0044] Comparative Example 2 Comparative Example 2 Compared with Example 1, in the process of preparing the composite heat stabilizer in Comparative Example 2, no vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) was added, and other conditions remained unchanged.
[0045] Comparative Example 3 Comparative Example 3 Compared with Example 1, in the process of preparing the composite thermal stabilizer in Comparative Example 3, 4,4-difluorobenzophenone was not added, and other conditions remained unchanged.
[0046] Comparative Example 4 Comparative Example 4 Compared with Example 1, in the process of preparing the composite thermal stabilizer in Comparative Example 4, spherical alumina was not added, and other conditions remained unchanged.
[0047] Comparative Example 5 Comparative Example 5 Compared with Example 1, in the process of preparing the hot box resin in Comparative Example 5, no composite heat stabilizer is added, and other conditions remain unchanged.
[0048] Comparative Example 6 Comparative Example 6 Compared with Example 1, in the process of preparing the hot box resin in Comparative Example 6, no bagasse extract was added, and other conditions remained unchanged.
[0049] The properties of the hot box resins prepared in Examples 1-5 and Comparative Examples 1-6 were tested. The room temperature tensile strength and free formaldehyde of the samples were tested according to JB / T 3828-2013, the thermal conductivity of the samples was tested according to ASTM E 1461-01, and the thermal stability of the samples was tested according to ASTM E 1131-08 (2014). The test results are shown in Table 1: Table 1
[0050] From the test results in Table 1, it can be seen that the hot box resin prepared in Examples 1-5 of the present invention has excellent strength, thermal conductivity, thermal stability and low free formaldehyde. From the comparison between Comparative Example 1 and Examples 1-5, it can be seen that the addition of hydrochloric acid methanol solution can effectively reduce the free formaldehyde of the hot box resin; from the comparison between Comparative Example 2 and Examples 1-5, it can be seen that the addition of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) can effectively improve the thermal stability of the hot box resin; from the comparison between Comparative Example 3 and Examples 1-5, it can be seen that the addition of 4,4-difluorobenzophenone can effectively improve the thermal conductivity of the hot box resin; from the comparison between Comparative Example 4 and Examples 1-5, it can be seen that the addition of spherical alumina can effectively improve the strength of the hot box resin; from the comparison between Comparative Example 5 and Examples 1-5, it can be seen that the addition of a composite thermal stabilizer can effectively improve the strength, thermal conductivity and thermal stability of the hot box resin; from the comparison between Comparative Example 6 and Examples 1-5, it can be seen that the addition of bagasse extract can effectively reduce the free formaldehyde of the hot box resin.
[0051] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0052] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high-strength hot box resin, characterized in that: The invention is composed of the following ingredients in parts by weight: 14-19 parts of phenolic compounds, 20-25 parts of aldehyde compounds, 6-12 parts of bagasse extract, 2-4 parts of sodium hydroxide solution, 2-5 parts of composite heat stabilizer, and 1-4 parts of coupling agent, wherein the bagasse extract is extracted from the bagasse using a hydrochloric acid methanol solution, and the composite heat stabilizer is prepared from polyetheretherketone and silicone gel.
2. The high-strength hot box resin according to claim 1, characterized in that: The preparation method of the bagasse extract comprises the following steps: Q1: The collected bagasse is crushed, sieved, and subjected to reflux extraction treatment with a mixed solution of benzene and ethanol. After the treatment, the bagasse is placed in a fume hood and vacuum dried to obtain a crude bagasse product; Q2: Place the crude sugarcane bagasse in a ball mill for grinding, place the ground crude sugarcane bagasse in a container, add hydrochloric acid methanol solution, seal, stir, centrifuge, wash and centrifuge, collect the supernatant, evaporate and concentrate, and freeze-dry to obtain the sugarcane bagasse extract.
3. The high-strength hot box resin according to claim 2, characterized in that: In the Q1, the sieve size is 60-80 mesh, the solid content of bagasse is ≥98%, the dosage ratio of bagasse, benzene and ethanol is (100-200) g: (1.8-2.2) L: 1 L, the reflux extraction treatment time is 24-28 h, the placement time in the fume hood is 12-15 h, the vacuum drying temperature is 40-50 ° C, and the time is 20-28 h.
4. The high-strength hot box resin according to claim 2, characterized in that: In the Q2, the rotation speed of the ball mill is 400-600 rpm, the grinding time is 22-26 h, the usage ratio of the ground crude bagasse and the hydrochloric acid methanol solution is (6-8) g: (150-200) mL, the concentration of the hydrochloric acid methanol solution is 1.36 mol / L, the stirring temperature is 25-32°C, the stirring time is 24-26 h, the centrifugal speed is 4000-6000 rpm, the temperature is 3-5°C, the time is 20-25 min, the centrifugation is washed and centrifuged with anhydrous methanol, the operation is repeated 3-5 times, and the freeze-drying temperature is -80 to -90°C for 24-30 h.
5. The high-strength hot box resin according to claim 1, characterized in that: The preparation method of the composite thermal stabilizer comprises the following steps: S1: Methyl vinyl silicone rubber and vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) are mixed to obtain a vinyl compound, which is then mixed with hydrogen-containing silicone oil, polymethyl hydrogen siloxane, a platinum catalyst and an inhibitor, and then placed in a vacuum mixer for mixing to obtain a silicone mixture; S2: mixing spherical aluminum oxide and zinc oxide to obtain a mixed filler, placing the mixed filler and the organic silicon mixture in a vacuum mixer to mix them to obtain an organic silicon gel; S3: After heating and melting diphenyl sulfone, 4,4-difluorobenzophenone, hydroquinone and sodium carbonate are added under the protection of helium, and after heating treatment, cooling and purification are performed to obtain composite polyetheretherketone; S4: Add the composite polyetheretherketone into a container containing cyclopentane sulfone, heat and stir under helium protection, then slowly add the silicone gel into the container, stir after evenly dispersing to obtain a composite mixture, quickly pour it into a mold, cool, and vacuum dry to obtain a composite thermal stabilizer.
6. The high-strength hot box resin according to claim 5, characterized in that: In the S1, the viscosity of the methyl vinyl silicone rubber is 500 Pa·s, the viscosity of the vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) is 8000 Pa·s, the mass ratio of the methyl vinyl silicone rubber to the vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane) is 2:(8-10), and the mass ratio of the vinyl complex, hydrogen-containing silicone oil, polymethyl hydrogen siloxane, platinum catalyst and inhibitor is (100-120):(5-6):(2.5- 2.8): (0.8-1): (0.3-0.35), the mixing speed is 500-600rpm, and the mixing time is 3-5min; in S2, the spherical diameter of spherical alumina is 2μm, the particle size of zinc oxide is 300nm, the mass ratio of alumina to zinc oxide is 2: (0.8-1.2), the mass ratio of the mixed filler to the silicone mixture is 1: (8-10), the speed of the vacuum mixer is 500-600rpm, and the mixing time is 5-10min.
7. The high-strength hot box resin according to claim 5, characterized in that: In S3, the heating melting temperature is 140-150°C, the mass ratios of diphenyl sulfone, 4,4-difluorobenzophenone, hydroquinone and sodium carbonate are (163.8-282.1): (140.47-184.29): (71.10-93.32): (82.56-108.24), and the heating treatment process is: heating at 190°C, 220°C, 250°C and 280°C for 40 minutes respectively. , and finally heated at 310°C for 30 minutes, and purified with acetone and water using a Soxhlet extractor; in S4, the mass ratio of composite polyetheretherketone, cyclopentane sulfone, and silicone gel is (10-12): (32-38): (8-10), the heating temperature is 280-300°C, the stirring time is 3-5h, the stirring time after uniform dispersion is 2-4h, the vacuum drying temperature is 80-90°C, and the time is 6-8h.
8. A method for preparing a high-strength hot box resin according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step (1): adding a phenolic compound, a bagasse extract and a sodium hydroxide solution into a container, placing a rotor, and then adding an aldehyde compound, heating the container to react, and obtaining a prepolymer product; Step (2): The prepolymer product, the composite thermal stabilizer and the coupling agent are mixed and stirred, reacted at a constant temperature, and distilled under reduced pressure to obtain a high-strength hot core box resin.
9. The method for preparing a high-strength hot box resin according to claim 8, characterized in that: In the step (1), the volume concentration of the sodium hydroxide solution is 15vt%, the heating temperature is 70-100°C, and the reaction time is 1-3h.
10. The method for preparing a high-strength hot box resin according to claim 8, characterized in that: In the step (2), the mixing and stirring time is 1-2 hours, the constant temperature reaction temperature is 60-70° C., and the reaction time is 1.5-3 hours.
Citation Information
Patent Citations
Thermally-stable two-component heat-conducting gel and preparation method thereof
CN115216154A
Alkaline phenolic resin for reclaimed sand and preparation method thereof
CN118325006A
Synthetic resin and process of making same
GB604599A