Shielding ink for producing variable-breadth electrolytic copper and use method of shielding ink

By using specially formulated shielding inks and UV curing technology, the problem of variable width in electrolytic copper foil production is solved, efficient and low-cost electric field distribution stability and energy saving are achieved, and the ink service life is extended.

CN118725633APending Publication Date: 2024-10-01NANJING LONGDIAN HUAXIN NEW ENERGY MATERIALS IND TECH RES INST CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410790531.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing electrolytic copper foil production technology cannot effectively realize variable width production, resulting in the cathode roller can only produce copper foil of the same width, resulting in a waste of materials and energy, and the thicker insulating glue coating increases material costs and affects the electric field distribution.

Method used

Use a method including 10-15% polyurethane acrylate, 20-50% cyclotrimethylolpropane methyl acrylate, 20-50% isobornyl acrylate, 0-5% trimethylolpropane triacrylate, 1-10% diphenyl( The shielding ink of 2,4,6-trimethylbenzoyl)phosphine oxide, 0-0.5% aluminum oxide and 0-0.5% wetting agent is prepared through stirring, grinding and UV curing steps to form an ultra-thin coating To adapt to the production of copper foil of different widths.

Benefits of technology

It achieves an ultra-thin coating that maintains the stability of electric field distribution without increasing material costs, reduces energy waste, improves production efficiency, and extends the ink life cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725633A_ABST
    Figure CN118725633A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic copper foils, in particular to shielding ink for producing variable-breadth electrolytic copper and a use method of the shielding ink, and the shielding ink comprises the following components: 10-15% of polyurethane acrylate, 20-50% of cyclotrimethylolpropane methylal acrylate (CTFA), 20-50% of isobornyl acrylate (IBOA), 0-5% of trimethylolpropane triacrylate (TMPTA), 1-10% of diphenyl (2, 4, 6-trimethyl-1, 3-pentanedione), 0-5% of a photoinitiator, 0-5% of a photoinitiator, 0-5% of a photoinitiator and 0-5% of a photoinitiator. The catalyst comprises the following components in percentage by weight: 0-0.5% of 2, 2, 6-trimethylbenzoyl) phosphine oxide, 0-0.5% of aluminum oxide and 0-0.5% of a wetting agent. According to the shielding ink for producing the variable-breadth electrolytic copper and the use method of the shielding ink, coating of insulating glue such as epoxy resin and the like is carried out in a shielding area 1 according to the CN 115094487A and the CN 114990644A, and the coating thickness is 0.5 mm. The problems that in the prior art, the larger the coating thickness is, the better the electroplating liquid corrosion resistance of insulating glue is, but the thicker coating thickness causes the increase of the material cost, influences the flow direction of the electroplating liquid in circulating operation, and further influences the electric field distribution and the crude foil quality are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytic copper foil, in particular to a shielding ink for variable width electrolytic copper production and a use method thereof. Background Art

[0002] Electrolytic copper is an efficient method for producing copper foil. It uses copper sulfate and sulfuric acid as electrolytes. Under certain current conditions, copper ions are reduced at the cathode to form pure copper foil. Impurities in crude copper, such as iron and zinc, which are more active than copper, will dissolve into ions (Zn and Fe) along with copper. Since these ions are less likely to precipitate than copper ions, the precipitation of these ions on the cathode can be avoided by properly adjusting the potential difference during electrolysis. The copper foil produced in this way is called "electrolytic copper" and has extremely high purity. It can be used in a wide range of applications and can be used to make electrical products.

[0003] Among them, electrolytic copper foil is the main material of the negative electrode current collector of lithium-ion batteries. The development of its production technology and the quality of its performance will directly affect the manufacturing process, performance and production cost of lithium-ion batteries. The current electrolytic foil production technology is to directly produce copper foil of the same width as the roller on the cathode roller. Therefore, the cathode roller of the same foil production machine can only produce copper foil of the same width, and then cut it according to the target width. During this period, the waste foil generated needs to be recycled, resulting in cost and energy waste;

[0004] In the existing technical solutions, there are two solutions for variable width copper foil. The first one, as described in CN 115094487A and CN 114990644 A, is to apply insulating glue such as epoxy resin in the shielding area 1, and the coating thickness is 0.5mm. The thicker the coating thickness, the better the corrosion resistance of the insulating glue to the electroplating solution will be. However, the thicker the coating thickness, the higher the material cost will be. At the same time, it will affect the flow direction of the circulating electroplating solution, thereby affecting the electric field distribution and the quality of the raw foil. In view of this problem, a shielding ink for variable width electrolytic copper production and a method of using the same are provided. Summary of the invention

[0005] The object of the present invention is to provide a shielding ink for variable width electrolytic copper production and a method of using the same to solve the problems raised in the above background technology. To achieve the above object, the present invention provides the following technical solution: a shielding ink for variable width electrolytic copper production, comprising the following components: 10-15% polyurethane acrylate, 20-50% cyclotrimethylolpropane methylal acrylate (CTFA), 20-50% isobornyl acrylate (IBOA), 0-5% trimethylolpropane triacrylate (TMPTA), 1%-10% diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 0-0.5% aluminum oxide, and 0-0.5% wetting agent.

[0006] Preferably, the method comprises the following steps:

[0007] Step 1: Pre-mixing by stirring: putting the polyurethane acrylate, cyclotrimethylolpropane formal acrylate, isobornyl acrylate, trimethylolpropane triacrylate and other raw materials into a stirring tank according to proportion, and performing preliminary stirring and mixing to ensure that various raw materials are fully mixed;

[0008] Step 2: Add photoinitiator and additives. During the stirring process, gradually add TPO photoinitiator and additives such as alumina, and continue to stir and mix until all raw materials are evenly dispersed in the ink;

[0009] Step 3, adding a wetting agent, adding an appropriate amount of the wetting agent, and continuing to stir and mix to ensure that the wetting agent is evenly distributed in the ink;

[0010] Step 4: Grinding and dispersing: transfer the stirred ink to a three-roll mill for grinding and dispersing to further refine the ink particles and improve the ink's stability and printing performance.

[0011] Step 5: Screening and filtering: Screening and filtering the prepared ink to remove impurities and particles;

[0012] Step six: quality inspection.

[0013] Preferably, the quality inspection includes viscosity testing, dryness testing, and stability testing.

[0014] Preferably, the viscosity test uses a viscometer to test the viscosity of the prepared ink.

[0015] Preferably, the drying test includes an initial drying test and a thorough drying test.

[0016] Preferably, the steps of the initial dry test include:

[0017] Step 1: Place a small amount of ink at 100 microns on the scraper groove and scrape it off quickly;

[0018] Step 2: Immediately turn on the stopwatch, and after 30 seconds, place a piece of paper with the bottom facing the zero mark flat on the groove;

[0019] Step 3: Press down quickly with your palm, peel off the paper, and measure the length of the unstained ink in millimeters;

[0020] Step 4: The measured value is the initial dryness, which is usually carried out at 25°C and relative humidity of 65±5%.

[0021] Preferably, the thorough test comprises:

[0022] Step 1: Place the ink at 100 microns on the scraper (the amount of ink is based on the amount of ink that fills the slot) and scrape it off quickly;

[0023] Step 2: Immediately cover it with a piece of scratch paper or plastic film, press it with your palm, and peel it off immediately;

[0024] Step 3: While timing, use a blank piece of paper to stick the ink until the ink is completely dry at 100 microns and does not stick to the paper;

[0025] Step 4, record the time from covering to non-stick paper, which is the thorough drying, and the test is also carried out at 25°C and relative humidity 65±5%.

[0026] Preferably, the grinding and dispersion is carried out at a rotation speed of 1500 r / min for 10-20 min.

[0027] Preferably, the viscosity of the prepared ink is 12 mpas.

[0028] A shielding ink for variable width electrolytic copper production and a method for using the same, comprising the following steps:

[0029] Step 1: polishing: polishing the outer circumference of the entire cathode roller using a polishing machine;

[0030] Step 2: Determine the shielding area, and use tooling to pre-bond a circle of tape at the convenient area between the ink and the copper foil at both ends of the cathode roller to protect the ink from exceeding the shielding area during the spraying process;

[0031] Step 3: Start the cathode roller, adjust the cathode roller speed and spray gun pressure to adjust the coating thickness and uniformity, and then remove the protective tape;

[0032] Step 4: Adjust the cathode roller speed to UV cure the ink in the UV lamp curing area.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] By adding 20-50% cyclotrimethylolpropane methylal acrylate (CTFA), 20-50% isobornyl acrylate (IBOA), and 0-5% trimethylolpropane triacrylate (TMPTA), three active monomers and active diluents can participate in the polymerization reaction, thereby avoiding the use of other volatile solvents to cause environmental pollution. The adhesion, crosslinking degree, temperature resistance, viscosity, etc. of the main resin can be adjusted. By adding 1%-10% diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO), the photoinitiator content can be appropriately increased or decreased according to the UV curing distance, curing time, etc., by adding aluminum oxide, it can be used to adjust the fluidity of the ink. By adding 0-0.5% wetting agent, it can be used to improve the wettability of the ink and improve adhesion, thereby solving the problem described in CN115094487 A and CN 114990644 A that insulating glue such as epoxy resin is applied in the shielding area 1, and the coating thickness is 0.5mm. The thicker the coating thickness, the better the corrosion resistance of the insulating glue to the electroplating solution will be. However, the thicker coating thickness will increase the material cost and affect the flow direction of the circulating electroplating solution, thereby affecting the electric field distribution and the quality of the raw foil. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a flowchart of the present invention;

[0036] Figure 2 This is a schematic diagram of the structure when the ink is applied to both ends of the cathode roller in the present invention;

[0037] Figure 3 The figure is a flowchart of the method for using the ink of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technical personnel in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] See also Figures 1 to 3The present invention provides a technical solution: a shielding ink for variable width electrolytic copper production, comprising the following components: 15% polyurethane acrylate, polyurethane acrylate is a special polymer material, and its molecules contain acrylic acid functional groups and urethane bonds, wear resistance and adhesion: PUA has the high wear resistance and adhesion of polyurethane, so that it performs well in various applications, flexibility and peel strength: the material shows excellent flexibility and high peel strength after curing, and can adapt to various complex application environments, low temperature resistance: it has excellent low temperature resistance and can maintain stable performance under low temperature conditions, optical properties and weather resistance: it combines the optical properties and weather resistance of polyacrylate, and is suitable for harsh environments such as outdoor, chemical resistance: it can maintain stability in corrosive media such as acids and alkalis, and has good chemical resistance, thermal stability and temperature resistance: it can maintain the stability of physical and chemical properties under high temperature conditions, and is suitable for industrial applications in high temperature environments, adjustability, the composition and chemical properties of polyurethane acrylate have a large adjustment space, and a variety of polyurethane acrylate prepolymers with different functional groups and characteristics can be synthesized, 50% cyclotrihydroxymethyl 10% diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, the content of photoinitiator can be appropriately increased or decreased according to UV curing distance, curing time, etc. 0.5% alumina, mainly used to adjust the flow of ink Moisture, 0.5% wetting agent, used to improve the wettability of ink, improve adhesion, the ink prepared by the above raw materials has a very low viscosity, <12mPaS, and the use of monomers with low viscosity and good dilution effect makes the ink have a very low viscosity, so that the spraying construction method can be adopted, and an ultra-thin ink coating is obtained after curing. The ink material has a high degree of cross-linking, and the spraying thickness only needs 50um to achieve stable adhesion in the electrolyte, which does not affect the electric field distribution during the electrolytic copper foil process. The ink material has a service life of 6 months, a long service life, and is stable in the electroplating solution. The ink is sprayed, which is convenient and fast.

[0041] Preferably, the method comprises the following steps:

[0042] Step 1: Pre-mixing by stirring: putting the polyurethane acrylate, cyclotrimethylolpropane formal acrylate, isobornyl acrylate, trimethylolpropane triacrylate and other raw materials into a stirring tank according to proportion, and performing preliminary stirring and mixing to ensure that various raw materials are fully mixed;

[0043] Step 2: Add photoinitiator and additives. During the stirring process, gradually add TPO photoinitiator and additives such as alumina, and continue to stir and mix until all raw materials are evenly dispersed in the ink;

[0044] Step 3, adding a wetting agent, adding an appropriate amount of the wetting agent, and continuing to stir and mix to ensure that the wetting agent is evenly distributed in the ink;

[0045] Step 4: Grinding and dispersing: transfer the stirred ink to a three-roll mill for grinding and dispersing to further refine the ink particles and improve the ink's stability and printing performance.

[0046] Step 5: Screening and filtering: Screening and filtering the prepared ink to remove impurities and particles;

[0047] Step 6: Quality inspection;

[0048] Stirring and mixing are performed using planetary mixers, butterfly paddle mixers, etc. Before stirring or mixing, check the cleanliness of the stirring equipment to ensure that no impurities remain.

[0049] Preferably, the quality inspection includes viscosity testing, dryness testing, and stability testing.

[0050] Preferably, the viscosity test uses a viscometer to test the viscosity of the prepared ink.

[0051] Preferably, the drying test includes an initial drying test and a thorough drying test.

[0052] Preferably, the steps of the initial dry test include:

[0053] Step 1: Place a small amount of ink at 100 microns on the scraper groove and scrape it off quickly;

[0054] Step 2: Immediately turn on the stopwatch, and after 30 seconds, place a piece of paper with the bottom facing the zero mark flat on the groove;

[0055] Step 3: Press down quickly with your palm, peel off the paper, and measure the length of the unstained ink in millimeters;

[0056] Step 4: The measured value is the initial dryness, which is usually carried out at 25°C and relative humidity of 65±5%.

[0057] Preferably, the thorough test comprises:

[0058] Step 1: Place the ink at 100 microns on the scraper (the amount of ink is based on the amount of ink that fills the slot) and scrape it off quickly;

[0059] Step 2: Immediately cover it with a piece of scratch paper or plastic film, press it with your palm, and peel it off immediately;

[0060] Step 3: While timing, use a blank piece of paper to stick the ink until the ink is completely dry at 100 microns and does not stick to the paper;

[0061] Step 4, record the time from covering to non-stick paper, which is the thorough drying, and the test is also carried out at 25°C and relative humidity 65±5%.

[0062] Preferably, the grinding and dispersion is carried out at a rotation speed of 1500 r / min for 20 min.

[0063] Preferably, the viscosity of the prepared ink is 12 mpas.

[0064] A shielding ink for variable width electrolytic copper production and a method for using the same, comprising the following steps:

[0065] Step 1: polishing: polishing the outer circumference of the entire cathode roller using a polishing machine;

[0066] Step 2: Determine the shielding area, and use tooling to pre-bond a circle of tape at the convenient area between the ink and the copper foil at both ends of the cathode roller to protect the ink from exceeding the shielding area during the spraying process;

[0067] Step 3: Start the cathode roller, adjust the cathode roller speed and spray gun pressure to adjust the coating thickness and uniformity, and then remove the protective tape;

[0068] Step 4: Adjust the cathode roller speed to UV cure the ink in the UV lamp curing area.

[0069] Example 2

[0070] See also Figures 1 to 3The present invention provides a technical solution: a shielding ink for variable width electrolytic copper production, comprising the following components: 10% polyurethane acrylate, polyurethane acrylate is a special polymer material, and its molecules contain acrylic acid functional groups and urethane bonds, wear resistance and adhesion: PUA has the high wear resistance and adhesion of polyurethane, so that it performs well in various applications, flexibility and peel strength: the material shows excellent flexibility and high peel strength after curing, and can adapt to various complex application environments, low temperature resistance: it has excellent low temperature resistance and can maintain stable performance under low temperature conditions, optical properties and weather resistance: it combines the optical properties and weather resistance of polyacrylate, and is suitable for harsh environments such as outdoor, chemical resistance: it can maintain stability in corrosive media such as acids and alkalis, and has good chemical resistance, thermal stability and temperature resistance: it can maintain the stability of physical and chemical properties under high temperature conditions, and is suitable for industrial applications in high temperature environments, adjustability, the composition and chemical properties of polyurethane acrylate have a large adjustment space, and a variety of polyurethane acrylate prepolymers with different functional groups and characteristics can be synthesized, 20% cyclotrimethylolpropane methylal propylene 1% diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, can appropriately increase or decrease the photoinitiator according to the UV curing distance, curing time, etc. Content, 0% aluminum oxide, 0% wetting agent, used to improve the wettability and adhesion of the ink. The viscosity of the ink prepared by the above materials is very low, <12mPaS. The use of monomers with low viscosity and good dilution effect makes the ink have a very low viscosity, so that the spraying construction method can be adopted. After curing, an ultra-thin ink coating is obtained. The ink material has a high degree of cross-linking, and the spraying thickness only needs 50um to achieve stable adhesion in the electrolyte, which does not affect the electric field distribution during the electrolytic copper foil process. The ink material has a service life of 6 months, a long service life, and is stable in the electroplating solution. The ink is sprayed, which is convenient and fast.

[0071] Preferably, the method comprises the following steps:

[0072] Step 1: Pre-mixing by stirring: putting the polyurethane acrylate, cyclotrimethylolpropane formal acrylate, isobornyl acrylate, trimethylolpropane triacrylate and other raw materials into a stirring tank according to proportion, and performing preliminary stirring and mixing to ensure that various raw materials are fully mixed;

[0073] Step 2: Add photoinitiator and additives. During the stirring process, gradually add TPO photoinitiator and additives such as alumina, and continue to stir and mix until all raw materials are evenly dispersed in the ink;

[0074] Step 3, adding a wetting agent, adding an appropriate amount of the wetting agent, and continuing to stir and mix to ensure that the wetting agent is evenly distributed in the ink;

[0075] Step 4: Grinding and dispersing: transfer the stirred ink to a three-roll mill for grinding and dispersing to further refine the ink particles and improve the ink's stability and printing performance.

[0076] Step 5: Screening and filtering: Screening and filtering the prepared ink to remove impurities and particles;

[0077] Step six: quality inspection.

[0078] Preferably, the quality inspection includes viscosity testing, dryness testing, and stability testing.

[0079] Preferably, the viscosity test uses a viscometer to test the viscosity of the prepared ink.

[0080] Preferably, the drying test includes an initial drying test and a thorough drying test.

[0081] Preferably, the steps of the initial dry test include:

[0082] Step 1: Place a small amount of ink at 100 microns on the scraper groove and scrape it off quickly;

[0083] Step 2: Immediately turn on the stopwatch, and after 30 seconds, place a piece of paper with the bottom facing the zero mark flat on the groove;

[0084] Step 3: Press down quickly with your palm, peel off the paper, and measure the length of the unstained ink in millimeters;

[0085] Step 4: The measured value is the initial dryness, which is usually carried out at 25°C and relative humidity of 65±5%.

[0086] Preferably, the thorough test comprises:

[0087] Step 1: Place the ink at 100 microns on the scraper (the amount of ink is based on the amount of ink that fills the slot) and scrape it off quickly;

[0088] Step 2: Immediately cover it with a piece of scratch paper or plastic film, press it with your palm, and peel it off immediately;

[0089] Step 3: While timing, use a blank piece of paper to stick the ink until the ink is completely dry at 100 microns and does not stick to the paper;

[0090] Step 4, record the time from covering to non-stick paper, which is the thorough drying, and the test is also carried out at 25°C and relative humidity 65±5%.

[0091] Preferably, the grinding and dispersion is carried out at a rotation speed of 1500 r / min for 10 min.

[0092] Preferably, the viscosity of the prepared ink is 12 mpas.

[0093] A shielding ink for variable width electrolytic copper production and a method for using the same, comprising the following steps:

[0094] Step 1: polishing: polishing the outer circumference of the entire cathode roller using a polishing machine;

[0095] Step 2: Determine the shielding area, and use tooling to pre-bond a circle of tape at the convenient area between the ink and the copper foil at both ends of the cathode roller to protect the ink from exceeding the shielding area during the spraying process;

[0096] Step 3: Start the cathode roller, adjust the cathode roller speed and spray gun pressure to adjust the coating thickness and uniformity, and then remove the protective tape;

[0097] Step 4: Adjust the cathode roller speed to UV cure the ink in the UV lamp curing area.

[0098] The above shows and describes the basic principles, main features and advantages of the present invention. Technical personnel in this industry should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not used to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A shielding ink for variable width electrolytic copper production, characterized in that: The invention comprises the following components: 10-15% polyurethane acrylate, 20-50% cyclotrimethylolpropane formal acrylate (CTFA), 20-50% isobornyl acrylate (IBOA), 0-5% trimethylolpropane triacrylate (TMPTA), 1%-10% diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 0-0.5% aluminum oxide and 0-0.5% wetting agent.

2. The shielding ink for variable width electrolytic copper production according to claim 1, characterized in that: The steps include: Step 1: Pre-mixing by stirring: putting the polyurethane acrylate, cyclotrimethylolpropane formal acrylate, isobornyl acrylate, trimethylolpropane triacrylate and other raw materials into a stirring tank according to proportion, and performing preliminary stirring and mixing to ensure that various raw materials are fully mixed; Step 2: Add photoinitiator and additives , during the stirring process, gradually add TPO photoinitiator and alumina and other additives, and continue to stir and mix until all the raw materials are evenly dispersed in the ink; Step 3, adding a wetting agent, adding an appropriate amount of the wetting agent, and continuing to stir and mix to ensure that the wetting agent is evenly distributed in the ink; Step 4: Grinding and dispersing: the stirred ink is transferred to a three-roll mill for grinding and dispersing to further refine the ink particles and improve the ink stability and printing performance; Step 5: Screening and filtering: Screening and filtering the prepared ink to remove impurities and particles; Step six: quality inspection.

3. The shielding ink for variable width electrolytic copper production according to claim 2, characterized in that: The quality inspection includes viscosity test, dryness test and stability test.

4. The shielding ink for variable width electrolytic copper production according to claim 3, characterized in that: The viscosity test uses a viscometer to test the viscosity of the prepared ink.

5. The shielding ink for variable width electrolytic copper production according to claim 3, characterized in that: The drying test includes an initial drying test and a thorough drying test.

6. The shielding ink for variable width electrolytic copper production according to claim 5, characterized in that: The steps of the initial dry test include: Step 1: Place a small amount of ink at 100 microns on the scraper groove and scrape it off quickly; Step 2: Immediately turn on the stopwatch, and after 30 seconds, place a piece of paper with the bottom facing the zero mark flat on the groove; Step 3: Press down quickly with your palm, peel off the paper, and measure the length of the unstained ink in millimeters; Step 4: The measured value is the initial dryness, which is usually carried out at 25°C and relative humidity of 65±5%.

7. The shielding ink for variable width electrolytic copper production according to claim 5, characterized in that: The thorough testing includes: Step 1: Place the ink at 100 microns on the scraper (the amount of ink is based on the amount of ink that fills the slot) and scrape it off quickly; Step 2: Immediately cover it with a piece of scratch paper or plastic film, press it with your palm, and peel it off immediately; Step 3: While timing, use a blank piece of paper to stick the ink until the ink is completely dry at 100 microns and does not stick to the paper; Step 4, record the time from covering to non-stick paper, which is the thorough drying, and the test is also carried out at 25°C and relative humidity 65±5%.

8. The shielding ink for variable width electrolytic copper production according to claim 2, characterized in that: The grinding and dispersion is carried out at a rotation speed of 1500 r / min for 10-20 min.

9. The shielding ink for variable width electrolytic copper production according to claim 2, characterized in that: The viscosity of the prepared ink is 12 mpas.

10. A shielding ink for variable width electrolytic copper production and a method of using the same, characterized in that: The steps include: Step 1: polishing: polishing the outer circumference of the entire cathode roller using a polishing machine; Step 2: Determine the shielding area, and use tooling to pre-bond a circle of tape at the convenient area between the ink and the copper foil at both ends of the cathode roller to protect the ink from exceeding the shielding area during the spraying process; Step 3: Start the cathode roller, adjust the cathode roller speed and spray gun pressure to adjust the coating thickness and uniformity, and then remove the protective tape; Step 4: Adjust the cathode roller speed to UV cure the ink in the UV lamp curing area.

Citation Information

Patent Citations

  • UV (Ultraviolet) offset halogen-free printing ink and preparation method thereof

    CN103525186A

  • UV ink-jet gloss oil and preparation method thereof

    CN111732873A

  • Novel shielding material for electrolytic copper foil and use method

    CN115094487A

  • UV curing ink-jet printing insulating ink and UV curing coating

    CN116445036A

  • Cathode shielding device with controllable width of electrolytic copper foil

    CN220555722U