Preparation method of temperature-sensitive color-changing biodegradable writable ink
By using components such as polyamide resin, nitrocellulose resin, and modified fumed silica in temperature-sensitive color-changing inks, combined with cobalt and nickel complexes, the problems of poor adhesion and printability of existing inks are solved, and high adhesion is achieved and thermosensitive color-changing biodegradable writeable ink with good printability.
Patent Information
- Application Number
- CN202410934510.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing temperature-sensitive color-changing inks have problems with poor adhesion, poor printability and poor degradability, making it difficult to meet the dual requirements of the food and beverage industry for writeability and environmental protection.
Polyamide resin and nitrocellulose resin are used as the main components, combined with environmentally friendly alcohol solvents and modified fumed silica, cobalt and nickel complexes are introduced to improve the adhesion and temperature-sensitive properties of the ink, and through surfactants and wetting Dispersants improve the uniformity and smoothness of the ink.
It achieves excellent adhesion and good printability of the temperature-sensitive color-changing biodegradable writeable ink, meeting the needs of the food and beverage industry for writeability and environmental protection.
Smart Images

Figure BDA0004940878730000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ink preparation, and in particular, relates to a method for preparing a thermosensitive color-changing biodegradable writing ink. Background Art
[0002] Writing ink is mainly used in bookmarks, sticky notes, etc. in our work, and label packaging in the food and beverage industry. The main purpose is to be able to write on the printed ink coating for identification and notes. Bookmarks and sticky notes in our work play such a role. In the food and beverage industry, in order to mark that the beverage is for personal consumption, a signature area is usually designed on the label, so the ink is required to be able to write. At the same time, it must also meet the current environmental protection requirements. As the material of the label is mostly biodegradable, the ink is also required to meet the requirements of biodegradability. Thermochromic makes the ink show different color changes under different temperature environments.
[0003] Chinese patent CN103305053A: discloses a thermochromic biodegradable water-based ink and its manufacturing process, characterized in that the components include a reversible thermochromic composite pigment, a carrier resin, a colloidal stabilizer, a water-soluble organic solvent, deionized water, a thickener, a surface wetting agent and other functional additives.
[0004] Chinese patent CN109251586A: discloses a preparation process of a temperature-sensitive color-changing printing ink. The specific preparation process is as follows: low-polymerization degree polyvinyl alcohol and bisphenol A epoxy resin react with toluene diisocyanate to obtain a composite resin solution; then add concentrated ammonia water thereto, react for 1 hour, heat to 70°C, add glutaraldehyde solution dropwise to the reaction container to obtain a viscous temperature-sensitive color-changing material liquid; then add hydroxy silicone oil, heat to 50°C, stir and react for 30 minutes, finally add defoamer, dispersant, varnish, and wetting agent, stir and mix at high speed for 3-5 minutes to obtain a temperature-sensitive color-changing ink.
[0005] Chinese patent CN117247698A: discloses a temperature-sensitive color-changing ink and a time-temperature indicating device. The raw materials for preparing the temperature-sensitive color-changing ink include, by mass, 20 to 35 parts of a connecting material, 5 to 15 parts of a reducing agent, and 40 to 60 parts of a solvent; wherein the reducing agent can undergo a redox color-changing reaction, and the reaction rate of the redox color-changing reaction is positively correlated with the temperature. In the above-mentioned temperature-sensitive color-changing ink, the reducing agent can undergo a redox color-changing reaction, and the rate of the redox color-changing reaction is positively correlated with the temperature, that is, the higher the temperature, the faster the rate of the redox color-changing reaction, and conversely, the lower the temperature, the slower the rate of the redox color-changing reaction, therefore, the degree of color change can be used to indicate the cumulative amount of heat received, and therefore, can be used to prepare a time-temperature indicating device. The time-temperature indicating device includes a substrate layer, an indicating layer and an isolation layer, wherein the indicating layer is obtained by printing the above-mentioned temperature-sensitive color-changing ink.
[0006] The inks prepared by the above patents and prior art have the problems of poor ink adhesion, poor printing properties, and poor degradability. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a temperature-sensitive color-changing biodegradable writing ink. The temperature-sensitive color-changing biodegradable writing ink is prepared by using polyamide resin, nitrocellulose resin, ethyl ester, isopropanol, ethanol, n-butanol, methyl ether, polyethylene wax powder, modified fumed silica, filler, organic bentonite, wetting dispersant, surfactant, and temperature-sensitive pigment.
[0008] Specifically, a method for preparing a thermosensitive color-changing biodegradable writing ink comprises the following steps:
[0009] S1: According to weight parts, weigh 20-30 parts of polyamide resin, 1-5 parts of nitrocellulose resin, 3-7 parts of ethyl acetate, 15-20 parts of isopropanol, 3-7 parts of ethanol, 3-7 parts of n-butanol, and 1-3 parts of methyl ether, and mix and stir for 20-60 minutes;
[0010] S2: Continue to add 0.5-2 parts of polyethylene wax powder, 1-5 parts of modified fumed silica, 1-5 parts of filler, 0.5-2 parts of organic bentonite, 0.5-2 parts of wetting dispersant, and 0.5-2 parts of surfactant, and mix and stir for 20-60 minutes;
[0011] S3: Finally, add 20-30 parts of temperature-sensitive pigment, stir for 50-100 minutes, filter, and obtain a temperature-sensitive color-changing biodegradable writing ink.
[0012] Preferably, the filler is one of calcium carbonate, magnesium carbonate, barium sulfate, aluminum hydroxide, lithopone and kaolin.
[0013] Preferably, the wetting and dispersing agent is one of B0K-F-501, B0K-F-502, B0K-F-505, B0K-F-508, and B0K-F-512.
[0014] Preferably, the surfactant is one of BOK-B-100, BOK-B-101, BOK-B-102, and BOK-B-103.
[0015] Preferably, the method for modifying fumed silica is:
[0016] T1: Add 50-100 parts of fumed silica, 3-6 parts of 3-isocyanate propyltrimethoxysilane, and 1000-1200 parts of ethanol into the reaction kettle, and stir at 40-60°C for 30-100 minutes under nitrogen protection;
[0017] T2: Add 20-30 parts of 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex and 0.006-0.06 parts of 3-iodo-2-hydroxybenzoic acid nickel complex to the reaction kettle of T1, add 2-5 parts of organic tin catalyst, stir at 60-70° C. for 30-100 minutes; filter and dry to obtain fumed silica loaded with cobalt complex, nickel complex and iodine substituent.
[0018] Preferably, the preparation method of the 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex is:
[0019] According to weight, 18-36 parts of 4-hydroxy-2,6-pyridinedicarboxylic acid, 29-58 parts of nickel nitrate hexahydrate and 300-400 parts of water are added into a stirring kettle, stirred at 40-50° C. for 30-60 minutes, and water is removed by distillation to obtain a 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex.
[0020] Preferably, the preparation method of the 3-iodo-2-hydroxybenzoic acid nickel complex is:
[0021] According to weight, 26-52 parts of 3-iodo-2-hydroxybenzoic acid, 20-40 parts of cobalt nitrate and 18-36 parts of water are added into a stirring kettle, stirred at 40-50° C. for 30-60 minutes, and water is removed by distillation to obtain 3-iodo-2-hydroxybenzoic acid nickel complex.
[0022] Preferably, the organic tin catalyst is one or more of dibutyltin dilaurate, stannous isooctanoate, and dibutyltin dodecylsulfide.
[0023] Compared with existing technologies:
[0024] 1. The present invention uses polyamide resin as the main connecting material and is combined with nitrocellulose to meet the requirements of good printing properties and drying speed of the ink; and the main raw materials for the production and synthesis of polyamide and nitrocellulose come from cotton, so they are biodegradable;
[0025] 2. The present invention adopts environmentally friendly alcohol solvents and esters as the main solvents, which not only ensures the solubility of the ink but also meets the current environmental protection standards;
[0026] 3. The present invention changes the particle size arrangement on the ink surface by adding modified fumed silica, so that the surface is arranged neatly and evenly to meet the requirements of being writable;
[0027] (1) Surface active sites: The introduction of cobalt and nickel complexes provides active chemical sites on the surface of silica;
[0028] (2) Thermochromic performance: The introduced cobalt complex and nickel complex have good compatibility with the temperature-sensitive pigment and also give the ink fine temperature-sensitive properties;
[0029] (3) Particle size adjustment: These complexes can affect the dispersion state and surface energy of the particles through interaction with the silica surface, thereby adjusting the size and distribution of the particles; the modified particles can be arranged more evenly on the substrate, reducing agglomeration, thereby improving the uniformity and smoothness of the coating;
[0030] (4) Improved adhesion: The introduction of complexes and iodine substituents increases the interaction between the ink and the substrate, improving adhesion.
[0031] 4. The temperature-sensitive color-changing biodegradable writing ink prepared by the present invention has excellent adhesion and good printability. DETAILED DESCRIPTION
[0032] The following embodiments are merely illustrative and non-restrictive, and should not be used to limit the scope of protection of the present invention.
[0033] The embodiments were tested according to QB / T1046-2012.
[0034] Example 1
[0035] A method for preparing a thermosensitive color-changing biodegradable writing ink, the operating steps of which are as follows:
[0036] S1: Weigh 20g polyamide resin PA6, 1g nitrocellulose resin, 3g ethyl acetate, 15g isopropanol, 3g ethanol, 3g n-butanol, and 1g methyl ether, and mix and stir for 20min;
[0037] S2: Continue to add 0.5g polyethylene wax powder, 1g modified fumed silica, 1g filler, 0.5g organic bentonite, 0.5g wetting dispersant, and 0.5g surfactant, and mix and stir for 20min;
[0038] S3: Finally, add 20 g of the temperature-sensitive pigment, stir for 50 min, and filter to obtain a temperature-sensitive color-changing biodegradable writing ink.
[0039] The filler is calcium carbonate.
[0040] The wetting and dispersing agent is B0K-F-501.
[0041] The surfactant is B0K-B-100.
[0042] The method for modifying fumed silica is:
[0043] T1: Add 50g of fumed silica, 3g of 3-isocyanate propyltrimethoxysilane and 1000g of ethanol into the reactor and stir at 40°C for 30 minutes under nitrogen protection;
[0044] T2: Add 20g of 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex and 0.006g of 3-iodo-2-hydroxybenzoic acid nickel complex to the reactor of T1, add 2g of organic tin catalyst, stir at 60°C for 30 minutes; filter and dry to obtain fumed silica loaded with cobalt complex, nickel complex and iodine substituent.
[0045] The preparation method of the 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex is:
[0046] 18 g of 4-hydroxy-2,6-pyridinedicarboxylic acid, 29 g of nickel nitrate hexahydrate, and 300 g of water were added to a stirring kettle, stirred at 40° C. for 30 minutes, and water was distilled off to obtain a 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex.
[0047] The preparation method of the 3-iodo-2-hydroxybenzoic acid nickel complex is:
[0048] 26 g of 3-iodo-2-hydroxybenzoic acid, 20 g of cobalt nitrate and 18 g of water were added to a stirring kettle, stirred at 40° C. for 30 minutes, and the water was distilled off to obtain 3-iodo-2-hydroxybenzoic acid nickel complex.
[0049] The organic tin catalyst is dibutyltin dilaurate.
[0050] Example 2
[0051] A method for preparing a thermosensitive color-changing biodegradable writing ink, the operating steps of which are as follows:
[0052] S1: Weigh 23g polyamide resin PA66, 2g nitrocellulose resin, 4g ethyl acetate, 16g isopropanol, 4g ethanol, 4g n-butanol, and 2g methyl ether, and mix and stir for 30min;
[0053] S2: Continue to add 1g polyethylene wax powder, 2g modified fumed silica, 2g filler, 1g organic bentonite, 1g wetting dispersant, and 1g surfactant, and mix and stir for 30min;
[0054] S3: Finally, add 24 g of temperature-sensitive pigment, stir for 60 min, and filter to obtain a temperature-sensitive color-changing biodegradable writing ink.
[0055] The filler is magnesium carbonate.
[0056] The wetting and dispersing agent is B0K-F-502.
[0057] The surfactant is BOK-B-101.
[0058] The method for modifying fumed silica is:
[0059] T1: Add 60g of fumed silica, 4g of 3-isocyanate propyltrimethoxysilane and 1050g of ethanol into the reactor and stir at 45°C for 50 minutes under nitrogen protection;
[0060] T2: Add 23g of 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex and 0.02g of 3-iodo-2-hydroxybenzoic acid nickel complex to the reactor of T1, add 3g of organic tin catalyst, stir at 65°C for 50 minutes; filter and dry to obtain fumed silica loaded with cobalt complex, nickel complex and iodine substituent.
[0061] The preparation method of the 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex is:
[0062] 24 g of 4-hydroxy-2,6-pyridinedicarboxylic acid, 36 g of nickel nitrate hexahydrate, and 340 g of water were added to a stirring kettle, stirred at 45° C. for 40 minutes, and water was distilled off to obtain a 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex.
[0063] The preparation method of the 3-iodo-2-hydroxybenzoic acid nickel complex is:
[0064] 34 g of 3-iodo-2-hydroxybenzoic acid, 25 g of cobalt nitrate and 22 g of water were added to a stirring kettle, stirred at 45° C. for 40 minutes, and water was distilled off to obtain 3-iodo-2-hydroxybenzoic acid nickel complex.
[0065] The organic tin catalyst is stannous isooctanoate.
[0066] Example 3
[0067] A method for preparing a thermosensitive color-changing biodegradable writing ink, the operating steps of which are as follows:
[0068] S1: Weigh 28g polyamide resin PA11, 4g nitrocellulose resin, 6g ethyl acetate, 18g isopropanol, 6g ethanol, 6g n-butanol, and 2g methyl ether, and mix and stir for 50min;
[0069] S2: Continue to add 1.5g polyethylene wax powder, 4g modified fumed silica, 4g filler, 1.5g organic bentonite, 1.5g wetting dispersant, and 1.5g surfactant, and mix and stir for 50min;
[0070] S3: Finally, add 28 g of the temperature-sensitive pigment, stir for 90 min, and filter to obtain a temperature-sensitive color-changing biodegradable writing ink.
[0071] The filler is barium sulfate.
[0072] The wetting and dispersing agent is B0K-F-505.
[0073] The surfactant is B0K-B-102.
[0074] The method for modifying fumed silica is:
[0075] T1: Add 90g of fumed silica, 5g of 3-isocyanate propyltrimethoxysilane and 1150g of ethanol into the reactor and stir at 55°C for 80 minutes under nitrogen protection;
[0076] T2: Add 28g of 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex and 0.04g of 3-iodo-2-hydroxybenzoic acid nickel complex to the reactor of T1, add 4g of organic tin catalyst, stir at 65°C for 80 minutes; filter and dry to obtain fumed silica loaded with cobalt complex, nickel complex and iodine substituent.
[0077] The preparation method of the 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex is:
[0078] 32 g of 4-hydroxy-2,6-pyridinedicarboxylic acid, 55 g of nickel nitrate hexahydrate, and 380 g of water were added to a stirring kettle, stirred at 45° C. for 50 minutes, and water was distilled off to obtain a 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex.
[0079] The preparation method of the 3-iodo-2-hydroxybenzoic acid nickel complex is:
[0080] 48 g of 3-iodo-2-hydroxybenzoic acid, 35 g of cobalt nitrate and 32 g of water were added to a stirring kettle, stirred at 45° C. for 50 minutes, and the water was distilled off to obtain 3-iodo-2-hydroxybenzoic acid nickel complex.
[0081] The organic tin catalyst is stannous isooctanoate.
[0082] Example 4
[0083] A method for preparing a thermosensitive color-changing biodegradable writing ink, the operating steps of which are as follows:
[0084] S1: Weigh 30g polyamide resin PA12, 5g nitrocellulose resin, 7g ethyl acetate, 20g isopropanol, 7g ethanol, 7g n-butanol, and 3g methyl ether, and mix and stir for 60min;
[0085] S2: Continue to add 2g polyethylene wax powder, 5g modified fumed silica, 5g filler, 2g organic bentonite, 2g wetting dispersant, and 2g surfactant, and mix and stir for 60min;
[0086] S3: Finally, add 30 g of the temperature-sensitive color pigment, stir for 100 min, and filter to obtain a temperature-sensitive color-changing biodegradable writing ink.
[0087] The filler is kaolin.
[0088] The wetting and dispersing agent is B0K-F-512.
[0089] The surfactant is BOK-B-103.
[0090] The method for modifying fumed silica is:
[0091] T1: Add 100 g of fumed silica, 6 g of 3-isocyanate propyltrimethoxysilane, and 1200 g of ethanol into the reactor, and stir at 60 ° C for 100 minutes under nitrogen protection;
[0092] T2: Add 30g of 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex and 0.06g of 3-iodo-2-hydroxybenzoic acid nickel complex to the reactor of T1, add 5g of organic tin catalyst, stir at 70°C for 100 minutes; filter and dry to obtain fumed silica loaded with cobalt complex, nickel complex and iodine substituent.
[0093] The preparation method of the 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex is:
[0094] 36 g of 4-hydroxy-2,6-pyridinedicarboxylic acid, 58 g of nickel nitrate hexahydrate, and 400 g of water were added to a stirring kettle, stirred at 50° C. for 60 minutes, and water was distilled off to obtain a 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex.
[0095] The preparation method of the 3-iodo-2-hydroxybenzoic acid nickel complex is:
[0096] 52 g of 3-iodo-2-hydroxybenzoic acid, 40 g of cobalt nitrate and 36 g of water were added to a stirring kettle, stirred at 50° C. for 60 minutes, and the water was distilled off to obtain 3-iodo-2-hydroxybenzoic acid nickel complex.
[0097] The organic tin catalyst is dibutyltin dodecylsulfide.
[0098] Comparative Example 1
[0099] In this example, the fumed silica was not modified, and the rest was the same as in Example 1.
[0100] Comparative Example 2
[0101] In this example, no 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex was added, and the other steps were the same as in Example 1.
[0102] Comparative Example 3
[0103] In this example, no 3-iodo-2-hydroxybenzoic acid nickel complex was added, and the other steps were the same as in Example 1.
[0104] Table 1 Test results of specific implementation scheme of this method:
[0105]
[0106] Through the data analysis of the above examples and comparative examples, the temperature-sensitive color-changing biodegradable writing ink prepared by the present invention has excellent adhesion and good printability.
[0107] Those skilled in the art should understand that the above embodiments are only exemplary embodiments, and various changes, substitutions and modifications may be made without departing from the spirit and scope of the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a thermosensitive color-changing biodegradable writing ink, the operating steps of which are: S1: According to weight parts, weigh 20-30 parts of polyamide resin, 1-5 parts of nitrocellulose resin, 3-7 parts of ethyl acetate, 15-20 parts of isopropanol, 3-7 parts of ethanol, 3-7 parts of n-butanol, and 1-3 parts of methyl ether, and mix and stir for 20-60 minutes; S2: Continue to add 0.5-2 parts of polyethylene wax powder, 1-5 parts of modified fumed silica, 1-5 parts of filler, 0.5-2 parts of organic bentonite, 0.5-2 parts of wetting dispersant, and 0.5-2 parts of surfactant, and mix and stir for 20-60 minutes; S3: Finally, add 20-30 parts of temperature-sensitive pigment, stir for 50-100 minutes, filter, and obtain a temperature-sensitive color-changing biodegradable writing ink.
2. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 1, characterized in that: The filler is one of calcium carbonate, magnesium carbonate, barium sulfate, aluminum hydroxide, lithopone and kaolin.
3. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 1, characterized in that: The wetting and dispersing agent is one of B0K-F-501, B0K-F-502, B0K-F-505, B0K-F-508, and B0K-F-512.
4. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 1, characterized in that: The surfactant is one of B0K-B-100, B0K-B-101, B0K-B-102 and B0K-B-103.
5. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 1, characterized in that: The method for modifying fumed silica is: T1: Add 50-100 parts of fumed silica, 3-6 parts of 3-isocyanate propyltrimethoxysilane, and 1000-1200 parts of ethanol into the reaction kettle, and stir at 40-60°C for 30-100 minutes under nitrogen protection; T2: Add 20-30 parts of 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex and 0.006-0.06 parts of 3-iodo-2-hydroxybenzoic acid nickel complex to the reaction kettle of T1, add 2-5 parts of organic tin catalyst, stir at 60-70° C. for 30-100 minutes; filter and dry to obtain fumed silica loaded with cobalt complex, nickel complex and iodine substituent.
6. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 5, characterized in that: The preparation method of the 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex is: According to weight, 18-36 parts of 4-hydroxy-2,6-pyridinedicarboxylic acid, 29-58 parts of nickel nitrate hexahydrate and 300-400 parts of water are added into a stirring kettle, stirred at 40-50° C. for 30-60 minutes, and water is removed by distillation to obtain a 4-hydroxy-2,6-pyridinedicarboxylic acid cobalt complex.
7. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 5, characterized in that: The preparation method of the 3-iodo-2-hydroxybenzoic acid nickel complex is: According to weight, 26-52 parts of 3-iodo-2-hydroxybenzoic acid, 20-40 parts of cobalt nitrate and 18-36 parts of water are added into a stirring kettle, stirred at 40-50° C. for 30-60 minutes, and water is removed by distillation to obtain 3-iodo-2-hydroxybenzoic acid nickel complex.
8. The method for preparing a thermosensitive color-changing biodegradable writing ink according to claim 5, characterized in that: The organic tin catalyst is one or more of dibutyltin dilaurate, stannous isooctanoate and dodecyl dibutyltin sulfide.
Citation Information
Patent Citations
Temperature-sensitive color-change water-based ink taking biodegradable resin as carrier and preparation process of ink
CN103305053A
Particle having attached halide group and method of making same
CN1309686A
Ink composition for oil marking pen
JP1998168374A
Oil-based ink composition for ball point pen
JP2015010156A
Thermochromic materials
US4028118A