Preparation method and application of high-thermal-conductivity SiO2-coated BNNS composite filler

By introducing hydroxyl groups on the surface of boron nitride and combining with silica to form SiO2@BNNS composite fillers, the problem of insufficient dispersion and affinity of thermally conductive fillers in electrical and electronic equipment is solved, and the heat dissipation performance and reliability of the equipment are significantly improved. Extended equipment life.

CN118725772APending Publication Date: 2024-10-01ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410870711.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing thermally conductive fillers such as boron nitride have high thermal conductivity but poor dispersion in electrical and electronic equipment, resulting in insufficient heat dissipation performance of the equipment, and insufficient affinity and dispersion in the matrix, affecting the reliability and life of the equipment.

Method used

By introducing hydroxyl groups on the surface of boron nitride and combining with silica, SiO2@BNNS composite filler is formed. Polyvinylpyrrolidone is used for surface modification to improve the dispersion and thermal conductivity of boron nitride in the matrix, and is added to the organic Silicone potting compound to improve thermal conductivity.

Benefits of technology

The SiO2@BNNS composite filler that achieves high thermal conductivity significantly improves the heat dissipation performance of electrical and electronic equipment, extends the reliability and life of the equipment, and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004921536380000031
    Figure BDA0004921536380000031
  • Figure BDA0004921536380000041
    Figure BDA0004921536380000041
  • Figure BDA0004921536380000042
    Figure BDA0004921536380000042
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic composite fillers, and discloses a preparation method and application of a high-thermal-conductivity SiO2-coated BNNS composite filler, and the preparation method comprises the following steps: (1) mixing 3-4 parts by mass of sodium hydroxide and 4-6 parts by mass of potassium hydroxide, dropwise adding 50-60 parts by mass of an ethanol solution, adding 1-2 parts by mass of boron nitride, and uniformly stirring; (2) pouring the mixed solution obtained in the step (1) into a reaction kettle for hydrothermal reaction; (3) after the reaction is completed, obtaining BNNS; (4) taking the BNNS and 0.1 to 0.2 part of polyvinylpyrrolidone, and dissolving the BNNS and the polyvinylpyrrolidone in 16 to 30 parts of absolute ethyl alcohol; and (5) mixing 0.4-0.7 part of ammonia water and 1.3-2.0 parts of tetraethoxysilane, mixing with the solution, drying, and grinding to obtain the composite filler. The composite filler not only can improve the dispersity in a matrix, but also can provide a large number of reaction sites, so that the thermal conductivity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inorganic composite fillers, and more specifically relates to a high thermal conductivity SiO 2 @BNNS Preparation method and application of composite filler. Background Art

[0002] As electrical and electronic equipment develops towards high power density, small size, light weight and high integration, the heat generated per unit volume of the equipment increases dramatically. The continuous accumulation of heat and the resulting temperature rise will accelerate the aging and failure of the insulating dielectric, greatly reducing the reliability and life of the electrical and electronic equipment. For electrical appliances, the reliability decreases by 10% for every 2°C above the rated temperature. For every 6°C increase in transformer winding temperature, the expected life is shortened by half. Therefore, it is necessary to further improve the heat dissipation performance of electrical and electronic equipment. However, improving the thermal conductivity of insulating materials is the fundamental way to enhance the heat dissipation capacity of electrical and electronic equipment. Common thermal conductive fillers include boron nitride, aluminum nitride, silicon nitride, aluminum oxide, magnesium oxide, etc. Boron nitride is a thermal conductive filler with high thermal conductivity, stable structure, high thermal conductivity (theoretical value is 1700-2000W / (m·K)), while maintaining insulation properties, low expansion coefficient, and acid and alkali corrosion resistance. However, boron nitride only has trace amounts of hydroxyl and amino groups on the edges and fewer reaction sites, so boron nitride has poor affinity with the matrix material. Therefore, its surface needs to be modified to enhance its affinity with the matrix and improve its dispersibility in the matrix. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a high thermal conductivity SiO 2 @BNNS composite filler preparation method and application. The present invention uses a strong alkaline solution to expand the interlayer spacing of the two-dimensional material boron nitride, and connects hydroxyl groups to the surface of the boron nitride; the introduction of hydroxyl groups on the surface of the boron nitride can not only improve the dispersibility of the boron nitride in the matrix, but also provide a large number of reaction sites to achieve highly flexible and highly specific chemical reactions, and obtain boron nitride nanosheets by high-speed separation in a centrifuge; the surface of the boron nitride nanosheets is modified by polyvinyl pyrrolidone, and then silicon dioxide and the boron nitride nanosheets are used to form SiO 2 @BNNS composite filler has better bonding and higher thermal conductivity. 2 @BNNS Composite fillers are added to silicone potting compounds to increase their thermal conductivity.

[0004] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0005] A high thermal conductivity SiO 2 The preparation method of the @BNNS composite filler, by weight, comprises the following steps:

[0006] (1) After mixing 3-4 parts of sodium hydroxide and 4-6 parts of potassium hydroxide, 50-60 parts of ethanol solution are added dropwise thereto, and 1-2 parts of boron nitride are added, and stirred evenly;

[0007] (2) pouring the mixed solution obtained in step (1) into a reaction kettle for hydrothermal reaction;

[0008] (3) After the reaction is completed, BNNS is obtained by centrifugation, drying, and grinding;

[0009] (4) dissolving the BNNS obtained in step (3) and 0.1-0.2 parts of polyvinyl pyrrolidone in 16-30 parts of anhydrous ethanol and stirring until the mixture is uniform;

[0010] (5) Mix 0.4-0.7 parts of ammonia water and 1.3-2.0 parts of ethyl orthosilicate, mix them with the solution obtained in step (4), stir them thoroughly, dry them, and grind them to obtain SiO 2 @BNNS composite filler.

[0011] Further preferably, in step (1), the mass concentration of the ethanol solution is 50%.

[0012] Further preferably, in step (1), the stirring is: stirring at room temperature, with a rotation speed of 400-600 r / min, and a continuous stirring time of 2-3 h.

[0013] Further preferably, in step (2), the conditions of the hydrothermal reaction are: temperature 140-160° C., reaction time 3-6 h. The hydrothermal reaction conditions are favorable for the introduction of hydroxyl groups on the surface of boron nitride, too low a temperature is unfavorable for the decomposition of alkaline substances, and too high a temperature will cause oxidation of metal hydroxides.

[0014] Further preferably, in step (3), the centrifugation conditions are: rotation speed 5000-6000 r / min, single centrifugation 8-10 min, and centrifugation 2-3 times.

[0015] Further preferably, in step (4), the mass concentration of the anhydrous ethanol is not less than 99.5%.

[0016] Further preferably, in step (4), the stirring is: stirring at room temperature, with a rotation speed of 400-600 r / min, and the stirring time is continuous for 2-3 h.

[0017] Further preferably, in step (5), the mass concentration of the ammonia water is 25-28%. The role of the ammonia water is to catalyze the hydrolysis of tetraethyl orthosilicate. Under the weak alkaline conditions of the ammonia water, the hydroxyl group directly reacts with tetraethyl orthosilicate through nucleophilic attack to form a five-coordinate transition state. The attack of the hydroxyl group makes the silicon nucleus negatively charged and causes the electron cloud to shift to the -OR group on the other side. Since the bond between the hydroxyl group and the silicon atom is stronger than the alcohol group, the Si-O bond of the group is weakened, and finally the alcohol group leaves the silicon atom to complete the hydrolysis reaction. The mass ratio of ammonia water to tetraethyl orthosilicate is 1:3. The amount of tetraethyl orthosilicate added is too little, and the silicon dioxide cannot completely cover the boron nitride. The amount of tetraethyl orthosilicate added is too much, and a thick layer of silicon dioxide is covered on the surface of the boron nitride, and the thermal conductivity of the composite material is reduced.

[0018] Further preferably, in step (5), the stirring is: stirring at room temperature, with a rotation speed of 400-600 r / min, and the stirring time is continuous for 12-24 h.

[0019] Technical solution 2 of the present invention: A high thermal conductivity SiO prepared by the above preparation method 2 @BNNS Application of composite fillers in silicone potting adhesives.

[0020] Further preferably, the application comprises the following steps: vinyl silicone oil, hydrogen-containing silicone oil, SiO 2 @BNNS composite filler and catalyst are mixed and cured at room temperature to obtain high thermal conductivity silicone potting glue, SiO 2 @BNNS The addition amount of composite filler is 5-20% of the total mass of vinyl silicone oil and hydrogen silicone oil.

[0021] A large amount of thermal conductive filler will cause the viscosity of the system to increase, which will seriously limit the application of the product. 2 @BNNS composite fillers can also be used in different materials such as plastics, thermal conductive rubber, thermal conductive plastics, thermal conductive silicone grease, thermal conductive double-sided tape, etc.

[0022] Compared with the prior art, the present invention has the following advantages: (1) simple process and high yield; (2) surface functionalization of BN is achieved to reduce interface phonon scattering and reduce interface thermal resistance; (3) delamination of ultra-thin BNNS is achieved to best utilize its extremely high in-plane thermal conductivity; (4) it has excellent thermal conductivity when used in silicone potting adhesive. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 For BN and SiO 2 XRD pattern of @BNNS. DETAILED DESCRIPTION

[0024] The technical content and effects of the present invention are further described in detail below in conjunction with the embodiments, but the present invention is not limited thereto.

[0025] Example 1

[0026] (1) 3 g of sodium hydroxide and 4 g of potassium hydroxide were mixed uniformly at room temperature, 50 g of 50% ethanol solution was added dropwise thereto, and 1 g of boron nitride (BN) was added and stirred uniformly.

[0027] (2) Pour the mixed solution obtained in step (1) into the inner tank of a reactor for hydrothermal reaction at 150° C. for 5 h.

[0028] (3) The solution obtained in step (2) is centrifuged at high speed in deionized water at a speed of 5000 r / min, a single centrifugation for 10 min, and centrifuged three times, so that the boron nitride is quickly exfoliated to form boron nitride nanosheets; then dried at 60° C. and ground to obtain BNNS.

[0029] (4) The BNNS obtained in step (3) and 0.1 g of polyvinyl pyrrolidone were dissolved in 16 g of anhydrous ethanol and stirred continuously until the mixture was uniformly mixed.

[0030] (5) Take 0.45 g of 25% ammonia water and 1.35 g of ethyl orthosilicate, mix them with the solution obtained in step (4) and stir them thoroughly, dry them at 60°C and grind them to obtain SiO 2 @BNNS composite filler.

[0031] Mix 10g vinyl silicone oil and 1g hydrogen silicone oil, add 0.55g raw material BN, pure BNNS, SiO 2 @BNNS composite filler, add 0.01g chloroplatinic acid catalyst, and cure at room temperature to obtain high thermal conductivity silicone potting glue. Test its thermal conductivity coefficient and repeat 3 times.

[0032] Table 1

[0033]

[0034]

[0035] like Figure 1 As shown, due to SiO 2 It is an amorphous structure, showing an amorphous distribution under X-ray diffraction, SiO 2 The (002) crystal plane has a broad diffraction peak at 20-30°, so compared with BN, SiO 2 The (002) peak intensity of @BNNS is reduced, while other characteristic peaks are similar. This is due to the SiO2 coated on the BN surface. 2 , which hinders the aggregation of BN.

[0036] As shown in Table 1, the filling amount of thermal conductive filler is 5% of the total amount of vinyl silicone oil and hydrogen silicone oil. It can be clearly seen that the thermal conductive filler is SiO 2 @BNNS's silicone potting compound has the highest thermal conductivity.

[0037] Example 2

[0038] (1) 3 g of sodium hydroxide and 4 g of potassium hydroxide were mixed at room temperature, 50 g of 50% ethanol solution was added dropwise thereto, and 1 g of BN was added and stirred evenly.

[0039] (2) Pour the mixed solution obtained in step (1) into the inner tank of a reactor for hydrothermal reaction at 150° C. for 5 h.

[0040] (3) The solution obtained in step (2) is centrifuged at high speed in deionized water at a speed of 5000 r / min, a single centrifugation for 10 min, and centrifuged three times, so that the boron nitride is quickly exfoliated to form boron nitride nanosheets; then dried at 60° C. and ground to obtain BNNS.

[0041] (4) The BNNS obtained in step (3) and 0.1 g of polyvinyl pyrrolidone were dissolved in 16 g of anhydrous ethanol and stirred continuously until the mixture was uniformly mixed.

[0042] (5) Take 0.45 g of 25% ammonia water and 1.35 g of ethyl orthosilicate, mix them with the solution obtained in step (4) and stir them thoroughly, dry them at 60°C and grind them to obtain SiO 2 @BNNS composite filler.

[0043] Mix 10g vinyl silicone oil and 1g hydrogen silicone oil, add 0.55g, 1.1g, 1.65g, and 2.2g of SiO 2 @BNNS composite filler, add 0.01g chloroplatinic acid catalyst, and cure at room temperature to obtain high thermal conductivity silicone potting glue. Test its thermal conductivity coefficient and repeat 3 times.

[0044] Table 2

[0045]

[0046]

[0047] As shown in Table 2, as the content of thermal conductive filler increases, the number of thermal conductive paths formed in the silicone potting compound increases, and the thermal conductivity of the silicone potting compound gradually increases. The filling amount of thermal conductive filler should not be too high, because a large amount of thermal conductive filler will cause the viscosity of the system to increase, which will seriously limit the application field of the product.

[0048] Example 3

[0049] (1) 3 g of sodium hydroxide and 4 g of potassium hydroxide were mixed at room temperature, 50 g of 50% ethanol solution was added dropwise thereto, and 1 g of BN was added and stirred evenly.

[0050] (2) The mixed solution obtained in step (1) was poured into the inner tank of a reactor for hydrothermal reaction. Experiments were conducted at a reaction temperature of 160° C. for 6 h and at a reaction temperature of 200° C. for 5 h.

[0051] (3) The solution obtained in step (2) is centrifuged at high speed in deionized water at a speed of 5000 r / min, a single centrifugation for 10 min, and centrifuged three times, so that the boron nitride is quickly exfoliated to form boron nitride nanosheets; then dried at 60° C. and ground to obtain BNNS.

[0052] (4) The BNNS obtained in step (3) and 0.1 g of polyvinyl pyrrolidone were dissolved in 16 g of anhydrous ethanol and stirred continuously until the mixture was uniformly mixed.

[0053] (5) Take 0.45 g of 25% ammonia water and 1.35 g of ethyl orthosilicate, mix them with the solution obtained in step (4) and stir them thoroughly, dry them at 60°C and grind them to obtain SiO 2 @BNNS composite filler.

[0054] 10 g of vinyl silicone oil and 1 g of hydrogenated silicone oil were mixed, and 0.55 g of SiO 2 @BNNS composite filler, thermal conductive filler filling amount 5%, add 0.01g chloroplatinic acid catalyst, and cure at room temperature to obtain high thermal conductive silicone potting glue. Test its thermal conductivity coefficient and repeat 3 times.

[0055] Table 3

[0056]

[0057]

[0058] The hydrothermal reaction conditions are favorable for the introduction of hydroxyl groups on the surface of boron nitride. Too low a temperature is not conducive to the decomposition of alkaline substances, as shown in Table 3. Too high a temperature will cause oxidation of metal hydroxides, thereby reducing the thermal conductivity.

[0059] Example 4

[0060] (1) 4 g of sodium hydroxide and 6 g of potassium hydroxide were mixed at room temperature, 50 g of 50% ethanol solution was added dropwise thereto, and 1.5 g of BN was added and stirred evenly.

[0061] (2) Pour the mixed solution obtained in step (1) into the inner tank of a reactor for hydrothermal reaction at 150° C. for 6 h.

[0062] (3) The solution obtained in step (2) is centrifuged at high speed in deionized water at a speed of 5000 r / min, a single centrifugation for 10 min, and centrifuged three times, so that the boron nitride is quickly exfoliated to form boron nitride nanosheets; then dried at 60° C. and ground to obtain BNNS.

[0063] (4) Dissolve the BNNS obtained in step (3) and 0.15 g of polyvinyl pyrrolidone in 25 g of anhydrous ethanol and continue stirring until the mixture is uniformly mixed.

[0064] (5) Take 0.45 g of 25% ammonia water and 1.35 g of ethyl orthosilicate, mix them with the solution obtained in step (4) and stir them thoroughly, dry them at 60°C and grind them to obtain SiO 2 @BNNS composite filler.

[0065] Mix 10g vinyl silicone oil and 1g hydrogen silicone oil, add 0.55g, 1.1g, 1.65g, and 2.2g of SiO 2 @BNNS composite filler, add 0.01g chloroplatinic acid catalyst, and cure at room temperature to obtain high thermal conductivity silicone potting glue. Test its thermal conductivity coefficient and repeat 3 times.

[0066] Table 4

[0067]

[0068]

[0069] As shown in Table 4, as the content of the thermally conductive filler increases, the number of thermally conductive paths formed in the silicone potting compound increases, and the thermal conductivity of the silicone potting compound gradually increases. In addition, compared with Example 2, Example 4 appropriately increases the composite ratio of BN, which will improve the thermal conductivity.

[0070] Comparative Example 1

[0071] (1) Dissolve 1 g of BN and 0.1 g of polyvinyl pyrrolidone in 16 g of anhydrous ethanol and continue stirring until the mixture is uniform.

[0072] (2) Take 0.45 g of 25% ammonia water and 1.35 g of ethyl orthosilicate, mix them with the solution obtained in step (1), stir them thoroughly, dry them at 60°C, and grind them to obtain SiO 2 @BN composite filler.

[0073] Mix 10g vinyl silicone oil and 1g hydrogen silicone oil, add 0.55g, 1.1g, 1.65g, and 2.2g of SiO2 @BN composite filler, add 0.01g chloroplatinic acid catalyst, and cure at room temperature to obtain high thermal conductivity silicone potting glue. Test its thermal conductivity coefficient and repeat 3 times.

[0074] Table 5

[0075]

[0076] As shown in Table 5, compared with Example 2, under the same addition amount, the SiO 2 The thermal conductivity of silicone potting adhesive prepared by @BN composite filler is much lower than that of SiO 2 The silicone potting compound prepared with @BNNS composite filler shows that the alkali solution treatment enlarges the interlayer spacing of BN and improves the thermal conductivity.

[0077] Comparative Example 2

[0078] (1) 3 g of sodium hydroxide and 4 g of potassium hydroxide were mixed uniformly at room temperature, 50 g of 50% ethanol solution was added dropwise thereto, and 1 g of BN was added and stirred uniformly.

[0079] (2) Pour the mixed solution obtained in step (1) into the inner tank of a reactor for hydrothermal reaction at 150° C. for 5 h.

[0080] (3) The solution obtained in step (2) is centrifuged at high speed in deionized water at a speed of 5000 r / min, a single centrifugation for 10 min, and centrifuged three times, so that the boron nitride is quickly exfoliated to form boron nitride nanosheets; then dried at 60° C. and ground to obtain BNNS.

[0081] (4) The BNNS obtained in step (3) and 0.1 g of polyvinyl pyrrolidone were dissolved in 16 g of anhydrous ethanol and stirred continuously until the mixture was uniformly mixed.

[0082] (5) Take 0.9 g of 25% ammonia water and 2.7 g of tetraethyl orthosilicate, mix them with the solution obtained in step (4) and stir them thoroughly, dry them at 60°C and grind them to obtain SiO 2 @BNNS composite filler.

[0083] 10g of vinyl silicone oil and 1g of hydrogenated silicone oil were mixed, and 0.55g, 1.1g, 1.65g, and 2.2g of SiO 2 @BNNS composite filler, add 0.01g chloroplatinic acid catalyst, and cure at room temperature to obtain high thermal conductivity silicone potting glue. Test its thermal conductivity coefficient and repeat 3 times.

[0084] Table 6

[0085]

[0086] As shown in Table 6, compared with Example 2, under the same addition amount, when the silicon dioxide composite ratio is too large, SiO 2 @The thermal conductivity of the silicone potting compound prepared by BNNS composite material decreases. This is because too much ethyl orthosilicate is added, which covers a thick layer of silicon dioxide on the surface of boron nitride, reducing the thermal conductivity of the composite material.

[0087] The above embodiments of the present invention are merely examples for illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all the embodiments here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for preparing a high thermal conductivity SiO2@BNNS composite filler, characterized in that: By mass, the method comprises the following steps: (1) After mixing 3-4 parts of sodium hydroxide and 4-6 parts of potassium hydroxide, 50-60 parts of ethanol solution are added dropwise thereto, and 1-2 parts of boron nitride are added, and stirred evenly; (2) pouring the mixed solution obtained in step (1) into a reaction kettle for hydrothermal reaction; (3) After the reaction is completed, BNNS is obtained by centrifugation, drying, and grinding; (4) dissolving the BNNS obtained in step (3) and 0.1-0.2 parts of polyvinyl pyrrolidone in 16-30 parts of anhydrous ethanol and stirring until the mixture is uniform; (5) Mix 0.4-0.7 parts of ammonia water and 1.3-2.0 parts of tetraethyl orthosilicate, mix the mixture with the solution obtained in step (4), stir the mixture thoroughly, dry the mixture, and grind the mixture to obtain a SiO2@BNNS composite filler.

2. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (1), the mass concentration of the ethanol solution is 50%.

3. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (1), the stirring is: stirring at room temperature, with a rotation speed of 400-600 r / min, and the stirring time is continuous for 2-3 h.

4. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (2), the conditions of the hydrothermal reaction are: temperature 140-160° C., reaction time 3-6 h.

5. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (3), the centrifugation conditions are: rotation speed 5000-6000r / min, single centrifugation 8-10min, centrifugation 2-3 times.

6. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (4), the mass concentration of the anhydrous ethanol is not less than 99.5%; the stirring is: stirring at room temperature, a rotation speed of 400-600 r / min, and a continuous stirring time of 2-3 h.

7. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (5), the mass concentration of the ammonia water is 25-28%.

8. The method for preparing the high thermal conductivity SiO2@BNNS composite filler according to claim 1, characterized in that: In step (5), the stirring is: stirring at room temperature, with a rotation speed of 400-600 r / min, and the stirring time is continuous for 12-24 hours.

9. Use of the SiO2@BNNS composite filler prepared by the preparation method according to any one of claims 1 to 8 in silicone potting adhesive.

10. The use according to claim 9, characterized in that: The method comprises the following steps: mixing vinyl silicone oil, hydrogenated silicone oil, SiO2@BNNS composite filler and catalyst, and curing at room temperature to obtain silicone potting glue, wherein the addition amount of SiO2@BNNS composite filler is 5-20% of the total mass of vinyl silicone oil and hydrogenated silicone oil.

Citation Information

Cited By

  • Composite heat-conducting, insulating and flame-retardant thermal interface material and preparation method thereof

    CN119592023A

  • Plasma-resistant perfluoroether rubber and preparation method thereof

    CN119955239A

  • A plasma-resistant perfluoroether rubber and its preparation method

    CN119955239B