Adhesive for aluminum-plastic film, preparation method of adhesive, aluminum-plastic film and lithium battery
Through the combination of polyolefin modified polymer and aliphatic isocyanate curing agent, combined with maleic anhydride, itaconic acid and linear alkyl anhydride-containing monomers, an adhesive film with excellent bonding strength and electrolyte corrosion resistance is formed. The problem of insufficient performance of aluminum-plastic film adhesive in the existing technology is solved, and the shell punching yield and heat sealing performance are significantly improved.
Patent Information
- Application Number
- CN202410670444.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing aluminum-plastic film adhesives to combine excellent bonding strength, electrolyte corrosion resistance and good heat sealing performance at the same time, resulting in poor yield of aluminum-plastic film punching.
It uses a combination of polyolefin modified polymer and aliphatic isocyanate curing agent, and is connected through chemical bonds of maleic anhydride, itaconic acid and linear alkyl anhydride-containing monomers to form an adhesive with excellent bonding strength and electrolyte corrosion resistance. Adhesive film, and promote the cross-linking reaction of the polymer through the initiator to improve the heat sealing performance of the adhesive layer.
It achieves high bonding strength, good electrolyte corrosion resistance and excellent heat sealing performance of the aluminum-plastic film, significantly improves the yield of punched shells, and ensures the stability and fluidity of the adhesive.
Smart Images

Figure BDA0004862504200000131 
Figure BDA0004862504200000151
Abstract
Description
Technical Field
[0001] The present application belongs to the field of lithium batteries, and specifically relates to an adhesive for aluminum-plastic film and a preparation method thereof, an aluminum-plastic film, and a lithium battery. Background Art
[0002] In recent years, with the development of new energy vehicles, 3C digital products, and microelectronics technology, the demand for lithium-ion batteries has continued to grow. As an important component of lithium-ion batteries, aluminum-plastic film can encapsulate electrolytes and protect batteries. The aluminum-plastic film includes a nylon layer, an outer adhesive layer, an aluminum foil layer, an inner adhesive layer, and a heat-sealing layer stacked in sequence. As an important component of aluminum-plastic film, adhesives need to have excellent bonding strength and resistance to electrolyte corrosion. The adhesive film formed by the adhesive has good heat-sealing properties, and the aluminum-plastic film has a good shell punching yield rate. However, the existing adhesives often cannot have the above multiple properties at the same time.
[0003] CN106459703.A discloses a polyolefin adhesive composition, which is composed of acid-modified chlorinated polyolefin, glycidylamine epoxy resin, and glycidyl ether epoxy resin, which are mixed with a curing agent and applied for use. Beneficial effects: The adhesive will not produce viscosity increase or gelation under long-term storage, and can maintain good application period characteristics. Even if it is bonded and aged at a low temperature below 80°C, which has little effect on the thermal shrinkage of the polyolefin substrate, it can also achieve good adhesion and chemical resistance between the polyolefin resin substrate and the metal substrate. However, the application performance of the adhesive, such as 85°C electrolyte resistance, is poor.
[0004] CN202010268184.5 discloses a method for synthesizing an adhesive for aluminum-plastic film. The method comprises: component A is prepared from maleic anhydride-modified polyolefin grafted bisphenol A type epoxy resin E44; component B is maleic anhydride-modified polyolefin grafted triglycidyl p-aminophenol; product C is prepared by copolymerization of terminal hydroxyl polybutadiene and hexamethylene diisocyanate. The above three components are blended, mixed with a curing agent, and then the adhesive is coated. Beneficial effect: The adhesive has excellent resistance to electrolyte corrosion and maintains more than 70% of the initial peel force after being immersed in an electrolyte at 85°C for 20 days. However, the heat sealing performance of the adhesive film formed by the adhesive is poor, and the deep punching yield of the aluminum-plastic film is poor. Summary of the invention
[0005] The present application aims to solve one of the technical problems in the related art at least to some extent.
[0006] In the first aspect of the present application, the present application proposes an adhesive for aluminum-plastic film, comprising: a polyolefin modified polymer and an aliphatic isocyanate curing agent, wherein the polyolefin modified polymer comprises a polyolefin material and a monomer chemically bonded to the polyolefin material, wherein the monomer comprises a maleic anhydride monomer, an itaconic acid monomer, and an anhydride monomer containing a linear alkyl group. Thus, the adhesive has excellent bonding strength and excellent resistance to electrolyte corrosion, the adhesive film formed by the adhesive has good heat sealing performance, and the aluminum-plastic film has a good shell punching yield rate.
[0007] According to some embodiments of the present application, the mass ratio of the polyolefin material, the maleic anhydride monomer, the itaconic acid monomer and the straight-chain alkyl-containing anhydride monomer is 100:(5-40):(5-15):(8-20). Thus, the content of the maleic anhydride monomer is moderate, and the weight average molecular weight and dropping point of the polyolefin modified polymer are better. The better weight average molecular weight is conducive to ensuring that the adhesive has good stability and fluidity, and the better dropping point is conducive to the mutual entanglement and wetting of the molecular chains in the adhesive.
[0008] According to some embodiments of the present application, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(10-30). Thus, the polyolefin modified polymer and the aliphatic isocyanate curing agent have a better cross-linking reaction effect, and the adhesive layer formed by the adhesive has a better cross-linking density and heat sealing performance.
[0009] According to some embodiments of the present application, the mass ratio of the polyolefin material, the maleic anhydride monomer, the itaconic acid monomer and the straight-chain alkyl-containing anhydride monomer is 100:(10-20):(7-12):(10-15). This is conducive to obtaining a polyolefin modified polymer with a better weight average molecular weight and dropping point.
[0010] According to some embodiments of the present application, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(15-25). Thus, the cross-linking reaction effect of the polyolefin modified polymer and the aliphatic isocyanate curing agent can be effectively improved, and the adhesive layer formed by the adhesive has a better cross-linking density and heat sealing performance.
[0011] According to some embodiments of the present application, the weight average molecular weight of the polyolefin modified polymer is 50000-120000, preferably 70000-100000. This is conducive to the adhesive having good stability and fluidity, and the polyolefin modified polymer and the aliphatic isocyanate curing agent have better compatibility.
[0012] According to some embodiments of the present application, the dropping point of the polyolefin modified polymer is 120° C.-145° C., preferably 125° C.-135° C. This is conducive to the mutual entanglement of molecular chains in the adhesive.
[0013] According to some embodiments of the present application, the polyolefin material includes a copolymer of ethylene and an α-olefin, wherein the α-olefin includes at least one of ethylene, propylene and 1-butene.
[0014] According to some embodiments of the present application, the straight-chain alkyl-containing acid anhydride monomer includes at least one acid anhydride group, and the carbon number of the straight-chain alkyl group of the straight-chain alkyl-containing acid anhydride monomer is 4 to 20. Thus, the adhesive has better stretchability, and the prepared aluminum-plastic film has better shell punching yield.
[0015] According to some embodiments of the present application, the straight-chain alkyl-containing anhydride monomer includes butyl succinic anhydride, 2-octenyl succinic anhydride, dodecenyl succinic anhydride and eicosene succinic anhydride, preferably 2-octenyl succinic anhydride.
[0016] According to some embodiments of the present application, the aliphatic isocyanate includes hexamethylene diisocyanate.
[0017] In the second aspect of the present application, the present application proposes a method for preparing the aforementioned adhesive for aluminum-plastic film, comprising: under the action of an initiator, a polyolefin material, a maleic anhydride monomer, an itaconic acid monomer and an acid anhydride monomer containing a linear alkyl group are subjected to a first mixing treatment to obtain a polyolefin modified polymer; and the polyolefin modified polymer and an aliphatic isocyanate are subjected to a second mixing treatment to obtain the adhesive. Thus, the preparation method is simple and easy to implement, low in price, and easy to realize industrial production.
[0018] According to some embodiments of the present application, the initiator includes at least one of di-tert-butyl perphthalate, tert-butyl hydroperoxide, diisopropyl peroxide, benzoyl peroxide, tert-butyl perbenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide and lauroyl peroxide.
[0019] According to some embodiments of the present application, the first mixing treatment is performed at a temperature of 115° C. to 120° C. for 3 h to 5 h. Thus, the reaction effect of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and anhydride monomer containing a linear alkyl group is good.
[0020] According to some embodiments of the present application, the second mixing treatment is performed at a temperature of 22° C. to 25° C. for 0.5 h to 2 h. This facilitates the cross-linking reaction between the anhydride group and the carboxylic acid group in the polyolefin modified polymer and the isocyanate group in the aliphatic isocyanate.
[0021] According to some embodiments of the present application, the molar ratio of the polyolefin material to the initiator is 100:(0.2-2.5), preferably 100:(0.5-1.0). Thus, the amount of primary free radicals generated by the initiator is moderate, which is conducive to obtaining a polyolefin modified polymer with a relatively good weight average molecular weight and dropping point.
[0022] In the third aspect of the present application, the present application proposes an aluminum-plastic film, wherein the aluminum-plastic film comprises a polypropylene film layer, an adhesive layer and an aluminum foil layer in sequence, wherein the adhesive layer comprises the adhesive described above, or the adhesive prepared by the method described above. Thus, the adhesive of the aluminum-plastic film has good heat-sealing performance, and the aluminum-plastic film has a good shell punching yield rate.
[0023] In the fourth aspect of the present application, the present application proposes a lithium battery, wherein the lithium battery comprises the aluminum-plastic film. Thus, the aluminum-plastic film, as an important component of the lithium-ion battery, can better encapsulate the electrolyte and protect the lithium battery. DETAILED DESCRIPTION
[0024] The terms "including" and "having" in the specification and claims of the present application and any modifications thereof are open expressions, that is, including the contents specified in the present application but not excluding other contents.
[0025] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.
[0026] In the first aspect of the present application, the present application proposes an adhesive for aluminum-plastic film, comprising: a polyolefin modified polymer and an aliphatic isocyanate curing agent, wherein the polyolefin modified polymer comprises a polyolefin material and a monomer chemically bonded to the polyolefin material, and the monomer comprises a maleic anhydride monomer, an itaconic acid monomer, and an acid anhydride monomer containing a linear alkyl group. Thus, the adhesive has excellent bonding strength and excellent resistance to electrolyte corrosion, the adhesive film formed by the adhesive has good heat sealing performance, and the aluminum-plastic film prepared by using the above adhesive film has a good shell punching yield rate.
[0027] The following is an explanation of how the aforementioned adhesive can achieve the aforementioned effects:
[0028] Maleic anhydride monomers, itaconic acid monomers and anhydride monomers containing linear alkyl groups are introduced into polyolefin materials. Due to the differences in the activity and structure of the monomers, the maleic anhydride monomers and the anhydride monomers containing linear alkyl groups will be connected to the tertiary carbon or secondary carbon of the long chain of the polyolefin molecule in a comb shape to form a branched chain, and the itaconic acid monomer will be connected to the two ends of the long chain of the polyolefin molecule in a linear homopolymer to form a straight chain. The straight chain and the branched chain work synergistically to form a dense network structure of the formed film. Maleic anhydride monomer and straight-chain alkyl-containing anhydride monomer include anhydride groups, itaconic acid monomer includes carboxylic acid groups, and aliphatic isocyanate curing agent includes isocyanate groups. The anhydride groups and carboxylic acid groups will cross-link with the isocyanate groups, so that the adhesive has excellent bonding strength and excellent resistance to electrolyte corrosion, which is beneficial to ensure that the adhesive layer formed by the adhesive has good heat sealing properties and the aluminum-plastic film has a good shell punching yield rate; in addition, aliphatic isocyanate is used as a curing agent, the anhydride groups, carboxylic acid groups and isocyanate groups have a better cross-linking reaction speed, and the adhesive has a better activation period.
[0029] In some embodiments, the mass ratio of the polyolefin material, the maleic anhydride monomer, the itaconic acid monomer and the linear alkyl-containing anhydride monomer is 100:(5-40):(5-15):(8-20).
[0030] Preferably, the mass ratio of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and straight-chain alkyl-containing anhydride monomer is 100:(10-20):(7-12):(10-15). For example, it can be 100:10:7:10, 100:15:7:10, 100:20:7:10, 100:15:8:10, 100:15:10:10, 100:15:12:10, 100:15:8:12, 100:15:8:14 or 100:15:8:15.
[0031] The mass ratio of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and anhydride monomer containing linear alkyl is controlled within the aforementioned range, the content of maleic anhydride monomer is moderate, the weight average molecular weight and dropping point of the polyolefin modified polymer are better, the better weight average molecular weight is conducive to ensuring that the adhesive has good stability and fluidity, and the better dropping point is conducive to the mutual entanglement and wetting of the molecular chains in the adhesive. In addition, it is conducive to avoiding too little content of maleic anhydride monomer, maleic anhydride monomer is not easy to collide and combine with polyolefin molecular free radicals, polyolefin molecular free radicals are prone to self-crosslinking, thereby causing the weight average molecular weight of the polyolefin modified polymer to be too large and the dropping point to be too large, and it is conducive to avoiding too much content of maleic anhydride monomer, too little polyolefin molecular free radicals, maleic anhydride monomer will produce a shielding effect, thereby causing the weight average molecular weight of the polyolefin modified polymer to be too large and the dropping point to be too large.
[0032] Furthermore, the mass ratio of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and straight-chain alkyl-containing anhydride monomer is controlled within the aforementioned range, and the content of the itaconic acid monomer is moderate. On the one hand, the itaconic acid monomer will be grafted to both ends of the polyolefin molecule in the form of a linear homopolymer, which can effectively improve the bonding strength and electrolyte corrosion resistance of the adhesive, and the adhesive layer formed by the adhesive has excellent density. On the other hand, the carboxylic acid group in the itaconic acid monomer and the isocyanate group in the aliphatic isocyanate curing agent have a better reaction speed, which can effectively reduce the curing temperature and curing time of the adhesive. In addition, it is helpful to avoid too little content of itaconic acid monomer, which makes it difficult to completely graft itaconic acid monomers on both ends of polyolefin molecules, resulting in poor density of the adhesive layer formed by the adhesive, poor bonding strength and electrolyte corrosion resistance of the adhesive, and it is helpful to avoid too much content of itaconic acid monomer and too many carboxylic acid groups. The reaction speed of the carboxylic acid group in the itaconic acid monomer and the isocyanate group in the aliphatic isocyanate curing agent is too fast, which can easily lead to a rapid increase in adhesive viscosity or gelation, and the adhesive has a short activation period, which leads to a significant increase in operation difficulty.
[0033] Furthermore, the mass ratio of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and anhydride monomer containing linear alkyl groups is controlled within the aforementioned range, and the content of the anhydride monomer containing linear alkyl groups is moderate, which is conducive to the mutual entanglement of the molecular chains in the adhesive. The adhesive has excellent bonding strength and resistance to electrolyte corrosion, the adhesive layer formed by the adhesive has excellent flexibility and excellent stretchability, and the aluminum-plastic film has a high yield rate of shell punching. In addition, it is helpful to avoid too little content of acid anhydride monomers containing straight-chain alkyl groups, the molecular chains in the adhesive are poorly entangled with each other, the adhesive layer formed by the adhesive has poor flexibility and poor stretchability, the aluminum-plastic film is prone to pinholes, cracks and other drawbacks during deep punching, and the aluminum-plastic film has a low yield rate of punching shells; it is helpful to avoid too much content of acid anhydride monomers containing straight-chain alkyl groups, the molecular chains in the adhesive are too entangled with each other, the flexibility of the adhesive layer formed by the adhesive is too high, delamination and aluminum leakage are prone to occur after peeling after heat sealing, the aluminum-plastic film has poor heat sealing performance and a low yield rate of punching shells.
[0034] In some embodiments, the weight average molecular weight of the polyolefin modified polymer is 50,000-120,000, preferably 70,000-100,000, for example, 70,000, 75,000, 80,000, 85,000, 90,000, 95,000 or 100,000.
[0035] The weight average molecular weight of the polyolefin modified polymer is controlled within the aforementioned range. The weight average molecular weight of the polyolefin modified polymer is moderate. A better weight average molecular weight is conducive to good stability and fluidity of the adhesive. The polyolefin modified polymer and the aliphatic isocyanate curing agent have better compatibility. The adhesive is easy to spread and wet between the polypropylene film layer and the aluminum foil layer, which can effectively improve the bonding strength and electrolyte corrosion resistance of the adhesive. The adhesive layer formed by the adhesive has better heat sealing performance, and the aluminum-plastic film has a higher shell punching yield rate. In addition, it is helpful to avoid the weight average molecular weight of the polyolefin modified polymer being too low, the cohesion of the polyolefin modified polymer being poor, the adhesive having poor bonding strength and heat resistance, the adhesive layer formed by the adhesive having poor heat sealing performance, and the aluminum-plastic film having a low shell punching yield rate, and it is helpful to avoid the weight average molecular weight of the polyolefin modified polymer being too high, the compatibility of the polyolefin modified polymer and the aliphatic isocyanate curing agent being poor, the adhesive having poor stability and fluidity, the adhesive being difficult to spread and wet between the polypropylene film layer and the aluminum foil layer, so that the adhesive has poor bonding strength and resistance to electrolyte corrosion, the adhesive layer formed by the adhesive has poor heat sealing performance, and the aluminum-plastic film has a low shell punching yield rate.
[0036] In some embodiments, the dropping point of the polyolefin modified polymer is 120°C-145°C, preferably 125°C-135°C, for example, 125°C, 126°C, 127°C, 128°C, 129°C, 130°C, 131°C, 132°C, 133°C, 134°C or 135°C.
[0037] Controlling the dropping point of the polyolefin modified polymer within the aforementioned range is beneficial to the mutual entanglement of the molecular chains in the adhesive, and is beneficial to improving the bonding strength between the polypropylene film layer and the aluminum foil layer. The adhesive layer formed by the adhesive has excellent heat sealing performance. When the aluminum-plastic film is formed by cold stamping, it has good ductility and can effectively avoid the occurrence of defects such as pinholes and cracks. In addition, it is helpful to avoid the dropping point of the polyolefin modified polymer being too low, and the adhesive layer formed by the adhesive is relatively soft, resulting in poor bonding strength and electrolyte corrosion resistance of the adhesive, and poor heat sealing performance of the adhesive layer. It is also helpful to avoid the dropping point of the polyolefin modified polymer being too high. On the one hand, it causes the adhesive to have poor stability and fluidity, and the adhesive is not easy to spread and wet between the polypropylene film layer and the aluminum foil layer, so that the adhesive has poor bonding strength and electrolyte corrosion resistance, and the adhesive layer formed by the adhesive has poor heat sealing performance. On the other hand, it causes the adhesive layer formed by the adhesive to be harder, and the aluminum-plastic film is prone to pinholes, cracks and other drawbacks when punching deep, and the aluminum-plastic film has a low punching yield rate.
[0038] In some embodiments, the polyolefin material includes a copolymer of ethylene and an α-olefin, wherein the α-olefin includes at least one of ethylene, propylene, and 1-butene.
[0039] In some embodiments, the straight-chain alkyl anhydride monomer includes at least one anhydride group, and the carbon number of the straight-chain alkyl group of the straight-chain alkyl anhydride monomer is 4-20. For example, the carbon number can be 4, 6, 8, 10, 12, 14, 16, 18 or 20. The carbon number of the straight-chain alkyl group of the straight-chain alkyl anhydride monomer will affect the stretchability of the adhesive, and thus, the straight-chain alkyl group of the straight-chain alkyl anhydride monomer has a moderate carbon number, and the adhesive has better stretchability.
[0040] In some embodiments, the linear alkyl group-containing anhydride monomer includes butyl succinic anhydride, 2-octenyl succinic anhydride, dodecenyl succinic anhydride, and eicosenyl succinic anhydride, preferably 2-octenyl succinic anhydride.
[0041] In some embodiments, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(10-30).
[0042] Preferably, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(15-25), for example, 100:15, 100:16, 100:17, 100:18, 100:19, 100:20, 100:21, 100:22, 100:23, 100:24 or 100:25.
[0043] The mass ratio of the polyolefin modified polymer and the aliphatic isocyanate curing agent is controlled within the aforementioned range, the content of the polyolefin modified polymer and the aliphatic isocyanate curing agent is moderate, the anhydride group, the carboxylic acid group and the isocyanate group have a better cross-linking reaction effect, the adhesive has better bonding strength and electrolyte corrosion resistance, the adhesive layer formed by the adhesive has better cross-linking density and heat sealing performance, and the aluminum-plastic film has a higher shell punching yield rate. In addition, it is beneficial to avoid too little content of the aliphatic isocyanate curing agent, resulting in poor cross-linking density of the adhesive layer formed by the adhesive, poor bonding strength and electrolyte corrosion resistance of the adhesive, and it is beneficial to avoid too much content of the aliphatic isocyanate curing agent, the aliphatic isocyanate curing agent is prone to self-cross-linking, resulting in greater brittleness and poor flexibility of the adhesive layer formed by the adhesive, which leads to the aluminum-plastic film being prone to pinholes, cracks and other drawbacks when punching deep, and the aluminum-plastic film has a lower shell punching yield rate.
[0044] In some embodiments, the aliphatic isocyanate includes hexamethylene diisocyanate.
[0045] In a second aspect of the present application, the present application proposes a method for preparing the aforementioned adhesive for aluminum-plastic film, comprising:
[0046] S100: Under the action of an initiator, a polyolefin material, a maleic anhydride monomer, an itaconic acid monomer and an acid anhydride monomer containing a linear alkyl group are subjected to a first mixing treatment to obtain a polyolefin modified polymer.
[0047] In this step, the initiator generates primary free radicals, which are dehydrogenated from the polyolefin molecules to form macromolecular free radicals. The dehydrogenated polyolefin molecules undergo grafting reaction with maleic anhydride monomers, itaconic acid monomers and anhydride monomers containing linear alkyl groups to obtain polyolefin modified polymers.
[0048] In some embodiments, the initiator comprises an organic peroxide.
[0049] In some embodiments, the initiator includes at least one of di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, diisopropylbenzene peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide and lauroyl peroxide. Preferably, di-tert-butyl peroxide is used.
[0050] In some embodiments, the molar ratio of the polyolefin material to the initiator is 100:(0.2-2.5),
[0051] Preferably, the molar ratio of the polyolefin material to the initiator is 100:(0.5-1.0), for example, it can be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9 or 100:1.0.
[0052] The molar ratio of the polyolefin material and the initiator is controlled within the aforementioned range, the content of the initiator is moderate, and the amount of the primary free radicals generated by the initiator is moderate, which is conducive to obtaining a polyolefin modified polymer with a relatively good weight average molecular weight and a dropping point. In addition, it is conducive to avoiding too little initiator content, resulting in less amount of primary free radicals generated by the initiator, and too large weight average molecular weight and dropping point of the polyolefin modified polymer, and it is conducive to avoiding too much initiator content, resulting in more amount of primary free radicals generated by the initiator, too many macromolecular free radicals formed by dehydrogenation on polyolefin molecules, and a greater probability of self-crosslinking of macromolecular free radicals, and too large weight average molecular weight and dropping point of the polyolefin modified polymer, resulting in poor stability and poor fluidity of the adhesive, and the adhesive is not easy to spread and wet between the polypropylene film layer and the aluminum foil layer, so that the adhesive has poor bonding strength and electrolyte corrosion resistance, the adhesive layer formed by the adhesive has poor heat sealing performance, and the aluminum-plastic film has a low shell punching yield rate.
[0053] In some embodiments, the feed ratio of the polyolefin material, the maleic anhydride monomer, the itaconic acid monomer and the linear alkyl-containing anhydride monomer is 100:(5-40):(5-15):(8-20).
[0054] Preferably, the feed ratio of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and straight-chain alkyl-containing anhydride monomer is 100:(10-20):(7-12):(10-15). For example, it can be 100:10:7:10, 100:15:7:10, 100:20:7:10, 100:15:8:10, 100:15:10:10, 100:15:12:10, 100:15:8:12, 100:15:8:14 or 100:15:8:15.
[0055] The mass ratio of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and straight-chain alkyl-containing anhydride monomer is controlled within the aforementioned range, and the prepared adhesive has excellent bonding strength and excellent resistance to electrolyte corrosion. The adhesive film formed by the adhesive has good heat-sealing properties, and the aluminum-plastic film has a good shell punching yield rate.
[0056] In some embodiments, the first mixing process is performed at a temperature of 115° C. to 120° C. for 3 h to 5 h.
[0057] As a specific example, the temperature of the first mixing treatment is 115° C., 116° C., 117° C., 118° C., 119° C. or 120° C., and the time of the first mixing treatment is 3 h, 3.5 h, 4 h, 4.5 h or 5 h.
[0058] The temperature and time of the aforementioned first mixing treatment are controlled within the aforementioned range. The temperature and time of the first mixing treatment are moderate, and the reaction effect of the polyolefin material, maleic anhydride monomer, itaconic acid monomer and acid anhydride monomer containing a straight-chain alkyl group is good. The maleic anhydride monomer and the acid anhydride monomer containing a straight-chain alkyl group will be connected to the tertiary carbon or secondary carbon of the long chain of the polyolefin molecule in a comb shape to form a branched chain, and the itaconic acid monomer will be connected to both ends of the long chain of the polyolefin molecule in a linear homopolymer.
[0059] In some embodiments, the polyolefin material, maleic anhydride monomer, itaconic acid monomer and anhydride monomer containing a linear alkyl group are subjected to a first mixing treatment in a solvent, wherein the solvent includes xylene, toluene and the like.
[0060] In some embodiments, step S100 further includes: adding the mixture after the first mixing treatment into a ketone reagent and cooling the mixture to precipitate a polyolefin modified polymer.
[0061] S200: performing a second mixing process on the polyolefin modified polymer and the aliphatic isocyanate to obtain an adhesive.
[0062] In this step, the polyolefin modified polymer and the aliphatic isocyanate are subjected to a second mixing treatment, and the anhydride groups and carboxylic acid groups in the polyolefin modified polymer will cross-link with the isocyanate groups in the aliphatic isocyanate, so that the adhesive has excellent bonding strength and excellent resistance to electrolyte corrosion, which is beneficial to ensure that the adhesive layer formed by the adhesive has good heat sealing properties and the aluminum-plastic film has a good shell punching yield.
[0063] In some embodiments, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(10-30).
[0064] Preferably, the feed ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(15-25), for example, 100:15, 100:16, 100:17, 100:18, 100:19, 100:20, 100:21, 100:22, 100:23, 100:24 or 100:25.
[0065] The feed ratio of the polyolefin modified polymer and the aliphatic isocyanate curing agent is controlled within the aforementioned range, the contents of the polyolefin modified polymer and the aliphatic isocyanate curing agent are moderate, the anhydride group, the carboxylic acid group and the isocyanate group have better cross-linking reaction effects, the adhesive has better bonding strength and resistance to electrolyte corrosion, the adhesive layer formed by the adhesive has better cross-linking density and heat-sealing properties, and the aluminum-plastic film has a higher yield rate of punching shells.
[0066] In some embodiments, the second mixing treatment is performed at a temperature of 22° C. to 25° C. for 0.5 h to 2 h.
[0067] As a specific example, the temperature of the second mixing treatment is 22° C., 22.5° C., 23° C., 23.5° C., 24° C., 24.5° C. or 25° C., and the time of the second mixing treatment is 0.5 h, 1 h, 1.5 h or 2 h.
[0068] The temperature and time of the second mixing treatment are controlled within the aforementioned range. The temperature and time of the second mixing treatment are moderate, which is conducive to the cross-linking reaction between the anhydride groups and carboxylic acid groups in the polyolefin modified polymer and the isocyanate groups in the aliphatic isocyanate.
[0069] In some embodiments, the second mixing process includes dissolving the polyolefin modified polymer in an organic solvent to form a mixed solution; slowly dropping aliphatic isocyanate into the mixed solution for mixing, and obtaining an adhesive after degassing.
[0070] Furthermore, the organic solvent includes a non-polar solvent and a polar solvent. The non-polar solvent includes cyclohexane, methylcyclohexane, etc., which can dissolve polyolefins, and the polar solvent includes ethyl acetate, butanone, acetone, etc., which can reduce the viscosity of the adhesive.
[0071] Furthermore, the degassing time is 2-10 minutes, thereby both fully removing the bubbles in the adhesive and having a high working efficiency.
[0072] In the third aspect of the present application, the present application proposes an aluminum-plastic film, wherein the aluminum-plastic film comprises a polypropylene film layer, an adhesive layer and an aluminum foil layer in sequence, wherein the adhesive layer comprises the adhesive described above, or the adhesive prepared by the method described above. Thus, the adhesive of the aluminum-plastic film has good heat-sealing performance, and the aluminum-plastic film has a good shell punching yield rate.
[0073] As an example, the present application provides a method for preparing an aluminum-plastic film, comprising the following steps:
[0074] S1: Apply the above-mentioned adhesive, or the adhesive prepared by the above-mentioned method, on the surface of the aluminum foil to form a bonding layer.
[0075] In some embodiments, the dry film thickness of the adhesive layer in step S1 is 2 micrometers to 4 micrometers.
[0076] S2: The aluminum foil coated with the adhesive layer and the polypropylene film are subjected to hot pressing and aging treatment in sequence to obtain an aluminum-plastic film.
[0077] In some embodiments, the temperature of the hot pressing lamination process is 90°C-110°C.
[0078] In some embodiments, the aging temperature is 30° C.-50° C., and the aging time is 0.5 day-2 days.
[0079] In the fourth aspect of the present application, the present application proposes a lithium battery, wherein the lithium battery comprises the aluminum-plastic film. Thus, the aluminum-plastic film, as an important component of the lithium-ion battery, can better encapsulate the electrolyte and protect the lithium battery.
[0080] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, unless otherwise explicitly stated, all reagents used in the following embodiments are commercially available or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0081] Example 1
[0082] The steps of preparing the adhesive for the aluminum plastic film include:
[0083] A copolymer of ethylene and 1-butene is used as a polyolefin material (hereinafter referred to as polyolefin resin), 2-octenyl succinic anhydride is used as an acid anhydride monomer containing a linear alkyl group, di-tert-butyl peroxide is used as an initiator, xylene is used as a solvent, and hexamethylene diisocyanate is used as an aliphatic isocyanate curing agent;
[0084] (1) Add polyolefin resin, maleic anhydride, 2-octenyl succinic anhydride, itaconic acid, di-tert-butyl peroxide and xylene into a reaction flask, heat the reaction flask until it is completely dissolved, then raise the temperature to 118° C., keep the temperature for 4 hours, cool down and pour into a ketone reagent to precipitate a polyolefin modified polymer, wherein the polyolefin resin is 100 parts by weight, maleic anhydride is 15 parts by weight, itaconic acid is 8 parts by weight, 2-octenyl succinic anhydride is 10 parts by weight, di-tert-butyl peroxide is 0.8 parts by weight, the weight average molecular weight of the polyolefin modified polymer is 95,000, and the dropping point of the polyolefin modified polymer is 130.2° C.;
[0085] (2) dissolving the aforementioned polyolefin modified polymer in a mixed solvent of cyclohexane and ethyl acetate at a dissolving temperature of 70° C., cooling to 24° C. after being completely dissolved, to obtain a mixed solution; then, slowly dropping hexamethylene diisocyanate into the mixed solution under stirring, stirring at high speed for 1 hour until uniform, and then standing for 5 minutes for degassing, to obtain an adhesive, wherein the hexamethylene diisocyanate is 20 parts by weight;
[0086] (3) The adhesive is coated on the surface of the aluminum foil, which has been treated with a trivalent chromium agent, and the dry film thickness of the adhesive is controlled to be 3 μm. The aluminum foil coated with the dry film of the adhesive and the CPP film are then laminated by hot pressing at a temperature of 100°C, and then placed in an oven at 40°C for aging for 1 day to obtain an aluminum-plastic film.
[0087] Example 2
[0088] The difference between Example 2 and Example 1 is only that:
[0089] 100 parts by weight of polyolefin resin, 5 parts by weight of maleic anhydride, 12 parts by weight of 2-octenylsuccinic anhydride, 8 parts by weight of itaconic acid, 0.6 parts by weight of di-tert-butyl peroxide, and 20 parts by weight of hexamethylene diisocyanate;
[0090] The weight average molecular weight of the polyolefin modified polymer is 105,000, and the dropping point of the polyolefin modified polymer is 135.2°C;
[0091] Other details are consistent with those in Example 1.
[0092] Example 3
[0093] The difference between Example 3 and Example 1 is only that:
[0094] 100 parts by weight of polyolefin resin, 40 parts by weight of maleic anhydride, 18 parts by weight of 2-octenylsuccinic anhydride, 8 parts by weight of itaconic acid, 1.6 parts by weight of di-tert-butyl peroxide, and 22 parts by weight of hexamethylene diisocyanate;
[0095] The weight average molecular weight of the polyolefin modified polymer is 58,000, and the dropping point of the polyolefin modified polymer is 122.6°C;
[0096] Other details are consistent with those in Example 1.
[0097] Example 4
[0098] The difference between Example 4 and Example 1 is only that:
[0099] 100 parts by weight of polyolefin resin, 8 parts by weight of maleic anhydride, 8 parts by weight of 2-octenylsuccinic anhydride, 6 parts by weight of itaconic acid, 0.5 parts by weight of di-tert-butyl peroxide, and 18 parts by weight of hexamethylene diisocyanate;
[0100] The weight average molecular weight of the polyolefin modified polymer is 115,000, and the dropping point of the polyolefin modified polymer is 143.0°C;
[0101] Other details are consistent with those in Example 1.
[0102] Example 5
[0103] The difference between Example 5 and Example 1 is only that:
[0104] 100 parts by weight of polyolefin resin, 7 parts by weight of maleic anhydride, 20 parts by weight of 2-octenylsuccinic anhydride, 7 parts by weight of itaconic acid, 0.9 parts by weight of di-tert-butyl peroxide, and 13 parts by weight of hexamethylene diisocyanate;
[0105] The weight average molecular weight of the polyolefin modified polymer is 71000, and the dropping point of the polyolefin modified polymer is 125.2°C;
[0106] Other details are consistent with those in Example 1.
[0107] Example 6
[0108] The difference between Example 6 and Example 1 is only that:
[0109] 100 parts by weight of polyolefin resin, 6 parts by weight of maleic anhydride, 9 parts by weight of 2-octenylsuccinic anhydride, 5 parts by weight of itaconic acid, 0.3 parts by weight of di-tert-butyl peroxide, and 18 parts by weight of hexamethylene diisocyanate;
[0110] The weight average molecular weight of the polyolefin modified polymer is 119,000, and the dropping point of the polyolefin modified polymer is 143.5°C;
[0111] Other details are consistent with those in Example 1.
[0112] Example 7
[0113] The difference between Example 7 and Example 1 is only that:
[0114] 100 parts by weight of polyolefin resin, 15 parts by weight of maleic anhydride, 9 parts by weight of 2-octenylsuccinic anhydride, 15 parts by weight of itaconic acid, 1.4 parts by weight of di-tert-butyl peroxide, and 10 parts by weight of hexamethylene diisocyanate;
[0115] The weight average molecular weight of the polyolefin modified polymer is 116,000, and the dropping point of the polyolefin modified polymer is 132.4°C;
[0116] Other details are consistent with those in Example 1.
[0117] Comparative Example 1
[0118] The difference between Comparative Example 1 and Example 1 is only that:
[0119] 100 parts by weight of polyolefin resin, 8 parts by weight of maleic anhydride, 10 parts by weight of 2-octenylsuccinic anhydride, 6 parts by weight of itaconic acid, 0.1 parts by weight of di-tert-butyl peroxide, and 14 parts by weight of hexamethylene diisocyanate;
[0120] The weight average molecular weight of the polyolefin modified polymer is 181000, and the dropping point of the polyolefin modified polymer is 155.2°C;
[0121] Other details are consistent with those in Example 1.
[0122] Comparative Example 2
[0123] The difference between Comparative Example 2 and Example 1 is only that:
[0124] 100 parts by weight of polyolefin resin, 6 parts by weight of maleic anhydride, 9 parts by weight of 2-octenylsuccinic anhydride, 6 parts by weight of itaconic acid, 2.7 parts by weight of di-tert-butyl peroxide, and 14 parts by weight of hexamethylene diisocyanate;
[0125] The weight average molecular weight of the polyolefin modified polymer is 173,000, and the dropping point of the polyolefin modified polymer is 150.2°C;
[0126] Other details are consistent with those in Example 1.
[0127] Comparative Example 3
[0128] The difference between Comparative Example 3 and Example 1 is only that:
[0129] 100 parts by weight of polyolefin resin, 45 parts by weight of maleic anhydride, 15 parts by weight of 2-octenylsuccinic anhydride, 10 parts by weight of itaconic acid, 1.0 parts by weight of di-tert-butyl peroxide, and 14 parts by weight of hexamethylene diisocyanate;
[0130] The weight average molecular weight of the polyolefin modified polymer is 45,000, and the dropping point of the polyolefin modified polymer is 115.5°C;
[0131] Other details are consistent with those in Example 1.
[0132] Comparative Example 4
[0133] The difference between Comparative Example 4 and Example 1 is only that:
[0134] 100 parts by weight of polyolefin resin, 2 parts by weight of maleic anhydride, 10 parts by weight of 2-octenylsuccinic anhydride, 9 parts by weight of itaconic acid, 0.4 parts by weight of di-tert-butyl peroxide, and 15 parts by weight of hexamethylene diisocyanate;
[0135] The weight average molecular weight of the polyolefin modified polymer is 165,000, and the dropping point of the polyolefin modified polymer is 152.0°C;
[0136] The rest are consistent with Example 1.
[0137] Comparative Example 5
[0138] The difference between Comparative Example 5 and Example 1 is only that:
[0139] 100 parts by weight of polyolefin resin, 15 parts by weight of maleic anhydride, 6 parts by weight of 2-octenylsuccinic anhydride, 8 parts by weight of itaconic acid, 0.6 parts by weight of di-tert-butyl peroxide, and 16 parts by weight of hexamethylene diisocyanate;
[0140] The weight average molecular weight of the polyolefin modified polymer is 100,000, and the dropping point of the polyolefin modified polymer is 134.2°C;
[0141] Other details are consistent with those in Example 1.
[0142] Comparative Example 6
[0143] The difference between Comparative Example 6 and Example 1 is only that:
[0144] 100 parts by weight of polyolefin resin, 15 parts by weight of maleic anhydride, 25 parts by weight of 2-octenylsuccinic anhydride, 8 parts by weight of itaconic acid, 1.0 parts by weight of di-tert-butyl peroxide, and 23 parts by weight of hexamethylene diisocyanate;
[0145] The weight average molecular weight of the polyolefin modified polymer is 98,000, and the dropping point of the polyolefin modified polymer is 131.0°C;
[0146] Other details are consistent with those in Example 1.
[0147] Comparative Example 7
[0148] The difference between Comparative Example 7 and Example 1 is only that:
[0149] 100 parts by weight of polyolefin resin, 10 parts by weight of maleic anhydride, 12 parts by weight of 2-octenylsuccinic anhydride, 3 parts by weight of itaconic acid, 0.6 parts by weight of di-tert-butyl peroxide, and 20 parts by weight of hexamethylene diisocyanate;
[0150] The weight average molecular weight of the polyolefin modified polymer is 108,000, and the dropping point of the polyolefin modified polymer is 136.2°C;
[0151] Other details are consistent with those in Example 1.
[0152] Comparative Example 8
[0153] The difference between Comparative Example 8 and Example 1 is only that:
[0154] 100 parts by weight of polyolefin resin, 10 parts by weight of maleic anhydride, 12 parts by weight of 2-octenylsuccinic anhydride, 18 parts by weight of itaconic acid, 1.0 parts by weight of di-tert-butyl peroxide, and 20 parts by weight of hexamethylene diisocyanate;
[0155] The weight average molecular weight of the polyolefin modified polymer is 115,000, and the dropping point of the polyolefin modified polymer is 134.9°C;
[0156] Other details are consistent with those in Example 1.
[0157] Comparative Example 9
[0158] The difference between Comparative Example 9 and Example 1 is only that:
[0159] 100 parts by weight of polyolefin resin, 15 parts by weight of maleic anhydride, 8 parts by weight of itaconic acid, 10 parts by weight of 2-octenylsuccinic anhydride, 0.8 parts by weight of di-tert-butyl peroxide, and 1 part by weight of hexamethylene diisocyanate;
[0160] The weight average molecular weight of the polyolefin modified polymer is 95,000, and the dropping point of the polyolefin modified polymer is 130.2°C;
[0161] Other details are consistent with those in Example 1.
[0162] Comparative Example 10
[0163] The difference between Comparative Example 10 and Example 1 is only that:
[0164] 100 parts by weight of polyolefin resin, 15 parts by weight of maleic anhydride, 8 parts by weight of itaconic acid, 10 parts by weight of 2-octenylsuccinic anhydride, 0.8 parts by weight of di-tert-butyl peroxide, and 40 parts by weight of hexamethylene diisocyanate;
[0165] The weight average molecular weight of the polyolefin modified polymer is 95,000, and the dropping point of the polyolefin modified polymer is 130.2°C;
[0166] Other details are consistent with those in Example 1.
[0167] The components of the adhesives of Examples 1-7 and Comparative Examples 1-10 are shown in Table 1.
[0168] Table 1
[0169]
[0170] The performance tests of the aluminum-plastic films prepared in Examples 1-7 and Comparative Examples 1-10 were conducted, specifically including:
[0171] (1) Bond strength test
[0172] The ambient temperature is (23±2)℃, the relative humidity is (50±10)%, and the aluminum-plastic film samples with a length greater than 150mm and a width of (15±0.1)mm are cut. The samples are tested using a universal material testing machine with a precision of 0.5. The initial distance between the fixtures is (100±5)mm, and the peeling is performed at a speed of (100±10)mm / min. The average force value is recorded.
[0173] (2) Heat sealing performance test
[0174] The aluminum plastic film was cut to obtain two rectangular test pieces of 15 mm wide × 200 mm long. After the two test pieces were overlapped in a way that the heat seal layers were in contact with each other, heat-sealed using a heat sealer at a temperature of 190°C and a sealing pressure of 0.5 MPa. The end area (unheat-sealed end) on the other side of the length direction of one of the two test pieces was clamped with the chuck of a tensile testing machine, and then peeled off at 90 degrees with an initial distance between the chucks of 100 mm and a tensile speed of 100 mm / min, and the heat seal strength per 15 mm width was measured. The whitish state and average force value of the peeled surface were recorded.
[0175] (3) Test of electrolyte corrosion resistance
[0176] Preparation of electrolyte: Ethylene carbonate, diethyl carbonate and dimethyl carbonate reagents are mixed in a ratio of 1:1:1, and lithium hexafluorophosphate is added to the mixture to prepare a solution with a lithium hexafluorophosphate substance content of 1.0 mol / L, which is the electrolyte. The free acid content of the electrolyte is not higher than 50 parts per million. The purity of the above reagents is analytical grade.
[0177] Cut the aluminum-plastic composite film into 15mm×100mm specimens, and place the specimens in a container filled with electrolyte. The electrolyte must completely immerse the specimens. After sealing the container, place it in an (85±2)℃ oven and keep it in an (85±2)℃ environment for 1 day. Take it out and let it cool naturally to room temperature. Take out the specimens one by one, wipe them clean, and immediately check the appearance of the specimens and test the bonding strength. Record the average force value.
[0178] (4) Shell punching yield
[0179] The aluminum-plastic film was cut and prepared into a three-dimensional shape (50 mm in length × 60 mm in width × 6 mm in depth, with flange) using a stamping die at an ambient temperature of (23±2)°C and a relative humidity of (50±10)%. The peripheral portions were heat-sealed with a heat sealer at a temperature of 190°C and a sealing pressure of 0.5 MPa to form a battery case, and the surface state was observed and the yield was calculated.
[0180] (5) Determination of weight average molecular weight
[0181] The molecular weight distribution of the solution polymer was determined by gel permeation chromatography, the standard substance was polystyrene resin, the mobile phase was tetrahydrofuran, the column temperature was 40°C, the flow rate was 1.0 ml / min, and the detector was a photodiode array detector. The test was carried out according to standard SH / T1759-2007.
[0182] (6) Determination of dropping point
[0183] Use a dropping point softening point tester, take an appropriate amount of the dried sample, add it to a metal grease cup in small amounts and multiple times, compact it repeatedly, use a blade to flatten the surface of the sample in one direction, and place it in a dry test tube for dropping point measurement; heat the temperature transfer liquid, and when the temperature rises to about 10°C lower than the specified lower limit of the dropping point, vertically put it into the test tube, continue heating, and adjust the heating rate to rise by 1.0-1.5°C per minute, record the temperature when the first drop of the molten sample leaves the metal grease cup, repeat the measurement 3 times, and take the average value.
[0184] (7) Evaluation of applicability
[0185] The pot life evaluation refers to the stability of the solution immediately after mixing the curing agent with the carboxylic acid or anhydride modified polyolefin resin or after a period of time. Good pot life characteristics mean that the viscosity of the solution increases little and can be stored for a long time. Poor pot life characteristics mean that the viscosity of the solution increases rapidly and even gelation occurs, making it difficult to apply and unable to be stored for a long time.
[0186] The performance test results of the aluminum-plastic films prepared in Examples 1-7 and Comparative Examples 1-10 are shown in Table 2.
[0187] Table 2
[0188]
[0189] Among them, * means that it is in a gel state and cannot be tested.
[0190] It can be seen from Table 2 that the performance of the aluminum-plastic film of the embodiment of the present application is significantly better than that of the aluminum-plastic film of the comparative example, indicating that the adhesive of the present application has excellent bonding strength, the aluminum-plastic film has good electrolyte corrosion resistance at 85°C, the film layer formed by the adhesive has good heat sealing performance, the aluminum-plastic film has a good shell punching yield, and the adhesive of the present application has a good application period, and the use effect can be achieved after aging at 40°C for 1 day, and can be used for the bonding of the aluminum foil layer and the heat sealing layer of the aluminum-plastic film.
[0191] Specifically, the amount of initiator added in Comparative Example 1-2 exceeds the range. If less initiator is added, the number of macromolecular free radicals generated from fewer initial free radicals is lower, resulting in less polar monomers grafted with polyolefins, too large a molecular weight, and too high a dropping point, resulting in high viscosity of the adhesive and inability to coat; if more initiator is added, the number of macromolecular free radicals generated is seriously excessive, while the number of grafted monomers is constant, which will greatly increase the probability of cross-linking between macromolecular free radicals, and the cross-linking reaction will dominate, resulting in too large a molecular weight and too high a dropping point, resulting in high viscosity of the adhesive and inability to coat.
[0192] The mass proportion of maleic anhydride in Comparative Examples 3-4 exceeds the range, the mass proportion of maleic anhydride is too large, the molecular weight is too small, and the dropping point is too low, resulting in poor bonding strength and electrolyte corrosion resistance, and low heat sealing performance of the aluminum-plastic film and shell punching yield. If the mass proportion of maleic anhydride is too small, the molecular weight is too high and the dropping point is too high, resulting in high viscosity of the adhesive and inability to apply.
[0193] In comparative examples 5-6, the mass proportion of 2-octenyl succinic anhydride exceeds the range, and the mass proportion of 2-octenyl succinic anhydride is too small, so the flexibility of the formed film is poor and the tensile performance is poor, which leads to poor bonding strength and electrolyte corrosion resistance, and a low aluminum-plastic film shell punching yield rate; if the mass proportion of 2-octenyl succinic anhydride is too large, the flexibility of the formed film is too large, which leads to poor bonding strength and electrolyte corrosion resistance, and a low aluminum-plastic film heat sealing performance and shell punching yield rate.
[0194] The mass proportion of isocyanate in Comparative Examples 7-8 exceeds the range. The mass proportion of isocyanate is too small. On the one hand, the carboxyl groups are not completely grafted onto the two ends of the polyolefin. On the other hand, the carboxylic acid content of the polyolefin modified polymer is too small, which cannot catalyze the reaction between the carboxyl and isocyanate groups well, resulting in poor density of the adhesive film, and thus poor bonding strength and resistance to electrolyte corrosion, and low heat sealing performance of the aluminum-plastic film and yield of punching shells. If the mass proportion of isocyanate is too large, the carboxylic acid content of the polyolefin modified polymer is too high, and at room temperature, it reacts quickly with the isocyanate group, resulting in a short activation period of the adhesive, which quickly becomes gel-like and cannot be coated.
[0195] The mass proportion of the curing agent in comparative examples 9-10 exceeds the range. If the mass proportion of the curing agent is too small, it will easily cause a low cross-linking density of the adhesive layer, resulting in poor bonding strength and electrolyte corrosion resistance, and poor heat sealing performance and shell punching yield of the aluminum-plastic film; if the mass proportion of the curing agent is too large, the adhesive layer formed by self-cross-linking of the excessive curing agent will be more brittle and less flexible, and the aluminum-plastic film will show a low shell punching yield.
[0196] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. An adhesive for aluminum-plastic film, characterized in that: include: A polyolefin modified polymer and an aliphatic isocyanate curing agent, wherein the polyolefin modified polymer comprises a polyolefin material and a monomer chemically bonded to the polyolefin material, wherein the monomer comprises a maleic anhydride monomer, an itaconic acid monomer and an anhydride monomer containing a linear alkyl group.
2. The adhesive according to claim 1, characterized in that The mass ratio of the polyolefin material, the maleic anhydride monomer, the itaconic acid monomer and the straight-chain alkyl-containing anhydride monomer is 100:(5-40):(5-15):(8-20); And / or, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(10-30).
3. The adhesive according to claim 2, characterized in that: The mass ratio of the polyolefin material, the maleic anhydride monomer, the itaconic acid monomer and the straight-chain alkyl-containing anhydride monomer is 100:(10-20):(7-12):(10-15); And / or, the mass ratio of the polyolefin modified polymer to the aliphatic isocyanate curing agent is 100:(15-25).
4. The adhesive according to any one of claims 1 to 3, characterized in that: The weight average molecular weight of the polyolefin modified polymer is 50,000-120,000, preferably 70,000-100,000; And / or, the dropping point of the polyolefin modified polymer is 120°C-145°C, preferably 125°C-135°C.
5. The adhesive according to any one of claims 1 to 3, characterized in that: The polyolefin material comprises a copolymer of ethylene and an α-olefin, wherein the α-olefin comprises at least one of ethylene, propylene and 1-butene; And / or, the acid anhydride monomer containing a linear alkyl group comprises at least one acid anhydride group, and the carbon number of the linear alkyl group of the acid anhydride monomer containing a linear alkyl group is 4-20; and / or, the straight-chain alkyl-containing anhydride monomer comprises butyl succinic anhydride, 2-octenyl succinic anhydride, dodecenyl succinic anhydride and eicosene succinic anhydride, preferably 2-octenyl succinic anhydride; And / or, the aliphatic isocyanate includes hexamethylene diisocyanate.
6. A method for preparing the adhesive for aluminum-plastic film according to any one of claims 1 to 5, characterized in that: include: Under the action of an initiator, a polyolefin material, a maleic anhydride monomer, an itaconic acid monomer and an acid anhydride monomer containing a linear alkyl group are subjected to a first mixing treatment to obtain a polyolefin modified polymer; The polyolefin modified polymer and aliphatic isocyanate are subjected to a second mixing process to obtain the adhesive.
7. The method according to claim 6, characterized in that The initiator comprises at least one of di-tert-butyl perphthalate, tert-butyl hydroperoxide, diisopropylbenzene peroxide, benzoyl peroxide, tert-butyl perbenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide and lauroyl peroxide.
8. The method according to claim 6 or 7, characterized in that: The first mixing treatment is carried out at a temperature of 115°C-120°C for 3h-5h; And / or, the second mixing treatment is carried out at a temperature of 22°C-25°C for 0.5h-2h; And / or, the molar ratio of the polyolefin material to the initiator is 100:(0.2-2.5), preferably 100:(0.5-1.0).
9. An aluminum-plastic film, characterized in that: The adhesive layer comprises a polypropylene film layer, a bonding layer and an aluminum foil layer in sequence, wherein the bonding layer comprises the adhesive according to any one of claims 1 to 5, or the bonding layer comprises the adhesive prepared by the method according to any one of claims 6 to 8.
10. A lithium battery, characterized in that: The invention comprises the aluminum-plastic film as claimed in claim 9.
Citation Information