Aluminum nitride seed crystal adhesive as well as preparation method and use method thereof
By combining aluminum nitride powder, aluminum oxide powder, polyethylene glycol and distilled water, an adhesive for aluminum nitride seed crystals is prepared, which solves the problem of unstable aluminum nitride seed crystal sticking in the existing technology. problem, achieving fast and stable aluminum nitride seed crystal installation.
Patent Information
- Application Number
- CN202410828151.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-01
AI Technical Summary
There is a lack of efficient adhesives in the preparation and application of existing aluminum nitride seed crystals, resulting in unstable adhesion and difficult installation during processing.
Using a combination of aluminum nitride powder, alumina powder, polyethylene glycol, anhydrous ethanol and distilled water, the aluminum nitride seed crystal paste is prepared by stirring, and magnetically stirred at a specific temperature and rotation speed to form a suitable Adhesive.
It achieves fast and stable pasting and installation of aluminum nitride seed crystals, simplifies the production process and facilitates industrial application.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum nitride seed crystal adhesives, and more specifically to an aluminum nitride seed crystal adhesive, a preparation method thereof, and a use method thereof. Background Art
[0002] Aluminum nitride (AlN) seed crystal is the basic material for the growth of aluminum nitride crystal. It has the characteristics of high strength, high volume resistivity, high insulation withstand voltage, small thermal expansion coefficient, and good matching with materials such as silicon. Aluminum nitride seed crystal has a wide range of application prospects in the semiconductor field, especially in the substrate material and packaging material of power semiconductor devices.
[0003] The preparation of aluminum nitride seed crystals usually involves complex chemical and physical processes. For example, AlN bulk single crystals can be prepared by physical vapor transport (PVT), which is a mainstream preparation method. In addition, boron nitride films can be prepared on the surface of single crystal silicon substrates by chemical vapor deposition (CVD), and then aluminum nitride films can be prepared on the surface of boron nitride films by metal organic chemical vapor deposition (MOCVD), thereby obtaining large-sized composite seed crystals.
[0004] The application of aluminum nitride seed crystal in the semiconductor field has attracted much attention because it not only has excellent physical and chemical properties, but also can form very small lattice mismatch and thermal mismatch with materials such as GaN and AlGaN. It is an ideal substrate material in the fields of deep ultraviolet detectors, deep ultraviolet LEDs, deep ultraviolet LDs and microwave high power.
[0005] In order to ensure that aluminum nitride seed crystals are processed and produced, an aluminum nitride seed crystal adhesive is required, which is the main medium for installing the aluminum nitride seed crystals. For this purpose, the present invention provides an aluminum nitride seed crystal adhesive. Summary of the invention
[0006] In order to overcome the above-mentioned defects of the prior art, the present invention provides an aluminum nitride seed crystal adhesive and a preparation method and a use method thereof to solve the problems existing in the above-mentioned background technology.
[0007] The present invention provides the following technical solution: an aluminum nitride seed crystal adhesive, comprising: 30-40 parts of aluminum nitride powder, 20-30 parts of aluminum oxide powder, 10-15 parts of polyethylene glycol, 5-10 parts of anhydrous ethanol and 10-50 parts of distilled water.
[0008] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0009] S1. Weigh 30-40 parts of aluminum nitride powder, 20-30 parts of aluminum oxide powder, 10-15 parts of polyethylene glycol, 5-10 parts of anhydrous ethanol and 10-50 parts of distilled water respectively;
[0010] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0011] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0012] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0013] S5, adding distilled water to the obtained first mixture;
[0014] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0015] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0016] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0017] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0018] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0019] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0020] Furthermore, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0021] Technical effects and advantages of the present invention:
[0022] The invention comprises the following steps: respectively weighing 30-40 parts of aluminum nitride powder, 20-30 parts of aluminum oxide powder, 10-15 parts of polyethylene glycol, 5-10 parts of anhydrous ethanol and 10-50 parts of distilled water; uniformly mixing the weighed aluminum nitride powder and aluminum oxide powder; pouring the uniformly mixed powder into the polyethylene glycol and stirring with a glass rod; pouring anhydrous ethanol and continuing to stir with the glass rod to obtain a first mixture; adding distilled water to the obtained first mixture; and magnetically stirring at a certain temperature to obtain an aluminum nitride seed crystal adhesive after the stirring is completed. The invention is conducive to rapid production of the aluminum nitride seed crystal adhesive and is convenient for production of the aluminum nitride seed crystal adhesive. DETAILED DESCRIPTION
[0023] The technical solutions in the present invention will be described clearly and completely below. In addition, the forms of the various structures described in the following embodiments are merely illustrative. The aluminum nitride seed crystal adhesive, preparation method and use method thereof involved in the present invention are not limited to the various structures described in the following embodiments. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] Embodiment 1
[0025] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0026] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0027] S1. Weigh 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0028] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0029] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0030] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0031] S5, adding distilled water to the obtained first mixture;
[0032] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0033] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0034] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0035] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0036] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0037] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0038] Furthermore, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0039] Embodiment 2
[0040] The invention provides an aluminum nitride seed crystal adhesive, comprising: 40 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0041] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0042] S1. Weigh 40 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0043] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0044] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0045] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0046] S5, adding distilled water to the obtained first mixture;
[0047] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0048] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0049] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0050] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0051] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0052] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0053] Furthermore, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0054] Embodiment 3
[0055] The invention provides an aluminum nitride seed crystal adhesive, comprising: 45 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0056] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0057] S1. Weigh 45 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0058] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0059] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0060] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0061] S5, adding distilled water to the obtained first mixture;
[0062] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0063] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0064] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0065] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0066] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0067] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0068] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0069] Embodiment 4
[0070] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 30 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0071] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0072] S1. Weigh 30 parts of aluminum nitride powder, 30 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0073] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0074] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0075] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0076] S5, adding distilled water to the obtained first mixture;
[0077] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0078] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0079] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0080] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0081] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0082] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0083] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0084] Embodiment 5
[0085] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 35 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0086] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0087] S1. Weigh 30 parts of aluminum nitride powder, 35 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0088] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0089] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0090] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0091] S5, adding distilled water to the obtained first mixture;
[0092] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0093] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0094] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0095] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0096] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0097] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0098] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0099] Embodiment 6
[0100] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 15 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0101] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0102] S1. Weigh 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 15 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0103] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0104] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0105] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0106] S5, adding distilled water to the obtained first mixture;
[0107] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0108] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0109] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0110] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0111] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0112] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0113] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0114] Embodiment 7
[0115] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 20 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water.
[0116] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0117] S1. Weigh 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 20 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0118] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0119] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0120] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0121] S5, adding distilled water to the obtained first mixture;
[0122] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0123] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0124] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0125] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0126] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0127] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0128] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0129] Embodiment 8
[0130] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 10 parts of anhydrous ethanol and 10 parts of distilled water.
[0131] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0132] S1. Weigh 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 10 parts of anhydrous ethanol and 10 parts of distilled water respectively;
[0133] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0134] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0135] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0136] S5, adding distilled water to the obtained first mixture;
[0137] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0138] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0139] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0140] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0141] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0142] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0143] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0144] Embodiment 9
[0145] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 50 parts of distilled water.
[0146] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0147] S1. Weigh 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 50 parts of distilled water respectively;
[0148] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0149] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0150] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0151] S5, adding distilled water to the obtained first mixture;
[0152] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0153] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0154] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0155] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0156] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0157] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0158] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0159] Embodiment 10
[0160] The invention provides an aluminum nitride seed crystal adhesive, comprising: 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 60 parts of distilled water.
[0161] A method for preparing an aluminum nitride seed crystal adhesive comprises the following steps:
[0162] S1. Weigh 30 parts of aluminum nitride powder, 20 parts of aluminum oxide powder, 10 parts of polyethylene glycol, 5 parts of anhydrous ethanol and 60 parts of distilled water respectively;
[0163] S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder;
[0164] S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod;
[0165] S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture;
[0166] S5, adding distilled water to the obtained first mixture;
[0167] S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
[0168] A method for using an aluminum nitride seed crystal adhesive comprises the following steps:
[0169] S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted;
[0170] S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air;
[0171] S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute;
[0172] S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
[0173] In a preferred embodiment, the magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.
[0174] The aluminum nitride seed crystals pasted with the aluminum nitride seed crystal paste are tested to determine whether the pasting is qualified, as shown in the following table.
[0175]
[0176] From the above table, it can be concluded that the proportions of the various components of the aluminum nitride seed crystal adhesive are: 30-40 parts of aluminum nitride powder, 20-30 parts of alumina powder, 10-15 parts of polyethylene glycol, 5-10 parts of anhydrous ethanol and 10-50 parts of distilled water, which can meet the qualified standards for adhesive bonding.
[0177] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An aluminum nitride seed crystal paste, It is characterized in that include: 30-40 parts of aluminum nitride powder, 20-30 parts of aluminum oxide powder, 10-15 parts of polyethylene glycol, 5-10 parts of anhydrous ethanol and 10-50 parts of distilled water.
2. A method for preparing an aluminum nitride seed crystal adhesive according to claim 1, Features: The following steps are involved: S1. Weigh 30-40 parts of aluminum nitride powder, 20-30 parts of aluminum oxide powder, 10-15 parts of polyethylene glycol, 5-10 parts of anhydrous ethanol and 10-50 parts of distilled water respectively; S2. Evenly mix the weighed aluminum nitride powder and aluminum oxide powder; S3, pouring the evenly mixed powder into polyethylene glycol and stirring with a glass rod; S4, pouring in anhydrous ethanol, and continuing to stir with a glass rod to obtain a first mixture; S5, adding distilled water to the obtained first mixture; S6. Perform magnetic stirring at a certain temperature to obtain an aluminum nitride seed crystal paste after the stirring is completed.
3. A method for using the aluminum nitride seed crystal adhesive according to claim 1, Features: The following steps are involved: S1. Prepare the aluminum nitride seed crystal and the pasting plate to be pasted; S2, wiping the aluminum nitride seed crystal pasting surface and the pasting position of the pasting plate with anhydrous ethanol to remove impurities adsorbed on the surface, and then placing it in a fan, so that the ethanol on the surface of the aluminum nitride seed crystal and the pasting plate can be quickly volatilized by the flow of air; S3, applying aluminum nitride seed crystal adhesive to the bonding position of the aluminum nitride seed crystal and the bonding plate and then leaving it for one minute; S4. Install the aluminum nitride seed crystal and the adhesive plate together, and cure them with a curing lamp to complete the installation of the aluminum nitride seed crystal.
4. A method for preparing an aluminum nitride seed crystal adhesive according to claim 2, Features: The magnetic stirring speed is 200-1000 r / min, the stirring time is 15-30 min, and the stirring temperature is 50-65 degrees Celsius.