Purple-light high-response green-light fluorescent material as well as preparation method and application thereof
Lu2SiO5:xEu2+'s purple-light high-response green fluorescent material solves the problem of existing WLEDs lacking green light components and blue light chips that are harmful to health. It achieves efficient green light emission and stable physical and chemical properties, meeting the needs of healthy lighting LEDs. needs.
Patent Information
- Application Number
- CN202410799795.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Existing white light-emitting diodes (WLEDs) lack green light components, have low color rendering index and high color temperature, which limits their application. In addition, incomplete conversion of blue light chips is harmful to human health and cannot meet the needs of high-quality, comfortable and healthy lighting.
Lu2SiO5:xEu2+ is used as a high-response green fluorescent material for purple light. It is synthesized through high-temperature solid-state method Al reduction and combined with Na2CO3 as a flux to prepare a green phosphor with a wide excitation band and stable physical and chemical properties, which can be used at 200-450nm. It effectively absorbs and emits strong green light at 504nm within the range, and is suitable for matching with a variety of chips.
It achieves green fluorescence performance that maintains more than 75% of the emission intensity under 400nm violet light excitation, meeting the needs of healthy lighting LEDs. It has a simple preparation process and is conducive to industrial production. It is suitable for white LEDs, sunlight-like LEDs and full-spectrum LEDs.
Smart Images

Figure CN118725865A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fluorescent material preparation, and in particular to a purple light high-response green light fluorescent material and a preparation method and application thereof. Background Art
[0002] As the fourth generation lighting source, white light emitting diodes (WLEDs) have attracted much attention in recent years due to their high efficiency, long life, and energy saving. Currently, commercial WLEDs are made by combining blue light GaN chips with yellow phosphor YAG:Ce 3+ However, due to the YAG:Ce 3+ Phosphors lack green and red components, and have a low color rendering index (CRI < 80) and high color temperature (> 4500K), which limit their application in WLEDs. In addition, blue light chips have the problem of incomplete conversion, which is harmful to human health, so it is called "blue light hazard". With the improvement of people's living standards, the demand for high-quality, comfortable and healthy lighting is increasing. A high-quality full-spectrum WLED that simulates the solar spectrum has been proposed to meet the demand for sunlight-like healthy lighting. This sunlight-like full-spectrum WLED mainly combines purple light chips with red, green and blue phosphors to achieve high color rendering, high light efficiency and adjustable color temperature sunlight-like healthy lighting LEDs. Green phosphor is one of the important components of tricolor phosphors. Designing and synthesizing green phosphors with strong absorption in the purple region plays an important role in healthy lighting. Summary of the invention
[0003] The purpose of the present invention is to provide a purple light high-response green light fluorescent material and a preparation method and application thereof.
[0004] The purpose of the present invention can be achieved by the following technical solution: a green light fluorescent material with high purple light response, the chemical expression of the fluorescent material is Lu2SiO5:xEu 2+ , where 0.01≤x≤0.05.
[0005] In the present invention, Lu2SiO5 is the matrix material, Eu 2+ Indicates that the matrix material is doped with Eu ions to partially replace Lu ions, and x represents the doped ion Eu 2+ The molar content of .
[0006] Preferably, x=0.01, 0.02, 0.03, 0.04 or 0.05.
[0007] Preferably, the purple light high-response green light fluorescent material is a powdery material.
[0008] Preferably, the excitation spectrum range of the purple light high-response green light fluorescent material covers 200 to 470 nm.
[0009] Further preferably, the excitation spectrum range of the purple light high-response green light fluorescent material covers 220 to 450 nm.
[0010] Preferably, the emission spectrum range of the purple light high-response green light fluorescent material covers 450 to 650 nm.
[0011] Further preferably, the emission spectrum range of the purple light high-response green light fluorescent material covers 450 to 600 nm.
[0012] Preferably, the emission intensity of the violet light highly responsive green fluorescent material under 400nm violet light excitation maintains 75% of the optimal emission.
[0013] Preferably, the purple light high-response green light fluorescent material can achieve strong green light emission with the emission center located at 504nm under the excitation of ultraviolet, purple and blue light in the range of 200 to 450nm.
[0014] A method for preparing the above-mentioned purple light high-response green light fluorescent material comprises the following steps:
[0015] (1) weighing raw material powders of a europium source compound, a lutetium source compound, and a silicon source compound according to a stoichiometric ratio, and grinding the raw material powders to uniformly mix them to obtain a mixture;
[0016] (2) sintering the mixture obtained in step (1) at high temperature in air to obtain a white powder after cooling;
[0017] (3) Grinding the white powder obtained in step (2) uniformly, then sintering it at high temperature by an Al reduction method, and obtaining the purple light high-response green light fluorescent material after cooling.
[0018] Preferably, in step (1), raw material powders of europium source compound, lutetium source compound, silicon source compound and sodium source compound are weighed and ground to uniformly mix the raw material powders to obtain a mixture.
[0019] Further preferably, the sodium source compound is Na2CO3, which serves as a flux.
[0020] Preferably, in step (1), according to the chemical formula of the fluorescent material (Lu2SiO5:xEu 2+ , where 0.01≤x≤0.05), on the basis of preparing various raw materials, 10-30wt% Na2CO3 is added as a flux to lower the reaction temperature.
[0021] Further preferably, 20 wt % Na 2 CO 3 is added as a flux.
[0022] Preferably, the europium source compound in step (1) is Eu2O3, the lutetium source compound is Lu2O3, and the silicon source compound is SiO2.
[0023] Preferably, the grinding time in step (1) is 5 to 120 minutes.
[0024] Preferably, the high temperature sintering conditions in step (2) are: sintering at 600-1400° C. for 1-10 hours.
[0025] Preferably, after high-temperature sintering in air in step (2), the mixture is further ground for 5 to 120 minutes to obtain a white powder.
[0026] Preferably, the cooling in step (2) refers to cooling to room temperature.
[0027] Preferably, the high temperature sintering conditions of step (3) are as follows: mixing the ground white powder with aluminum powder, and sintering at 500-1300° C. for 0.5-15 hours under vacuum conditions.
[0028] Further preferably, during the high temperature sintering in step (3), the system pressure is maintained at 0 MPa.
[0029] Further preferably, the mass ratio of the white powder to the aluminum powder is (0.25-0.35):1.
[0030] More preferably, the mass ratio of the white powder to the aluminum powder is 0.3:1.
[0031] More preferably, the ground white powder is mixed with aluminum powder and then sintered in a tube furnace.
[0032] More preferably, the ground white powder is mixed with aluminum powder and placed in a crucible, and the crucible is placed in a vacuum tube furnace, evacuated, and sintered at 750-1300° C. for 1-8 hours.
[0033] An application of the above-mentioned green light fluorescent material with high response to purple light is to use the above-mentioned green light fluorescent material with high response to purple light for healthy lighting.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The phosphor of the present invention is synthesized by Al reduction using a high-temperature solid-phase method for the first time, and has a wide excitation band, an effective absorption range covering 200 to 450 nm, and an emission center position at 504 nm;
[0036] 2. The phosphor of the present invention is Eu 2+ The doped oxide-based green light-emitting phosphor has the advantages of stable physical and chemical properties and is synthesized by solid phase method. Its preparation process is simple and is conducive to industrial production.
[0037] 3. The phosphor of the present invention is a broad excitation green phosphor, which is a new type of Eu doped 2+ Fluorescent materials have the advantages of stable physical and chemical properties. At the same time, the phosphor can be prepared by conventional solid-phase reaction method. Using Na2CO3 as flux can reduce the reaction temperature and avoid affecting its luminous intensity. It has the characteristics of simple preparation process and is conducive to industrial production.
[0038] 4. The phosphor of the present invention can be well matched with various existing ultraviolet and purple light chips, and maintains about 75% of the optimal emission intensity under excitation at 400nm. It has excellent luminous performance and meets the needs of the commercial market. It is suitable for the application of purple light-excited white light LEDs, purple light-excited solar light LEDs, purple light-excited full-spectrum LEDs and other healthy lighting LEDs. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a photoexcitation-emission spectrum of a purple light high-response green light phosphor for healthy lighting according to Examples 1-3 of the present invention. DETAILED DESCRIPTION
[0040] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0041] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0042] Example 1
[0043] This embodiment provides a method for preparing a purple light high-response green light phosphor for healthy lighting, the steps are:
[0044] 1. Weigh 1 g of Lu2O3, Eu2O3 and SiO2 raw material powders according to the stoichiometric ratio (the mass ratio of each raw material is Lu2O3:SiO2:Eu2O3=0.8621:0.1302:0.0078), and add 20 wt% of Na2CO3.
[0045] 2. Grind the above raw material mixture in an agate mortar for 30 to 60 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible, calcine it at 1200°C in air for 8 hours, then cool it to room temperature and grind it again for 30 to 60 minutes. Place it in an Al-reducing atmosphere and calcine it at 1000°C for 6 hours. Cool it to room temperature to obtain the target product.
[0046] 3. Use fluorescence spectrometer (HITACHI F-7500) to test the spectral properties of the phosphor in the system, such as Figure 1 As shown. The results show that the phosphor of this system has a wide excitation band, with a peak value near 370nm and a high spectral peak, which can match well with the commercial ultraviolet light chip. Under the excitation of 370nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (450-650nm) with a peak value at 504nm.
[0047] The ultraviolet excited Eu obtained in this example 2+ The general formula of doped green light emitting phosphor is Lu2SiO5:xEu 2+ , x is 0.01.
[0048] Example 2
[0049] This embodiment provides a method for preparing a purple light high-response green light phosphor for healthy lighting, the steps are:
[0050] 1. Weigh 1 g of Lu2O3, Eu2O3 and SiO2 raw material powders according to the stoichiometric ratio (the mass ratio of each raw material is Lu2O3:SiO2:Eu2O3=0.8505:0.1338:0.0157), and add 20 wt% of Na2CO3.
[0051] 2. Grind the above raw material mixture in an agate mortar for 30 to 60 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible, calcine it at 1250°C in air for 8 hours, then cool it to room temperature and grind it again for 30 to 60 minutes. Place it in an Al-reducing atmosphere and calcine it at 1050°C for 6 hours. Cool it to room temperature to obtain the target product.
[0052] 3. Use fluorescence spectrometer (HITACHI F-7500) to test the spectral properties of the phosphor in the system, such as Figure 1 As shown. The results show that the phosphor of this system has a wide excitation band, with a peak value near 370nm and a high spectral peak, which can match well with the commercial ultraviolet light chip. Under the excitation of 370nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (450-650nm) with a peak value at 504nm.
[0053] The ultraviolet excited Eu obtained in this example 2+ The general formula of doped green light emitting phosphor is Lu2SiO5:xEu 2+ , x is 0.02.
[0054] Example 3
[0055] This embodiment provides a method for preparing a purple light high-response green light phosphor for healthy lighting, the steps are:
[0056] 1. Weigh 1 g of Lu2O3, Eu2O3 and SiO2 raw material powders according to the stoichiometric ratio (the mass ratio of each raw material is Lu2O3:SiO2:Eu2O3=0.8411:0.1351:0.0237), and add 20 wt% of Na2CO3.
[0057] 2. Grind the above raw material mixture in an agate mortar for 30 to 60 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible, calcine it at 1150°C in air for 6 hours, then cool it to room temperature and grind it again for 30 to 60 minutes. Place it in an Al-reducing atmosphere and calcine it at 1100°C for 4 hours. Cool it to room temperature to obtain the target product.
[0058] 3. Use fluorescence spectrometer (HITACHI F-7500) to test the spectral properties of the phosphor in the system, such as Figure 1 As shown. The results show that the phosphor of this system has a wide excitation band, with a peak value near 370nm and a high spectral peak, which can match well with the commercial ultraviolet light chip. Under the excitation of 370nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (450-650nm) with a peak value at 504nm.
[0059] The ultraviolet excited Eu obtained in this example 2+ The general formula of doped green light emitting phosphor is Lu2SiO5:xEu 2+ , x is 0.03.
[0060] Example 4
[0061] This embodiment provides a method for preparing a purple light high-response green light phosphor for healthy lighting, the steps are:
[0062] 1. Weigh 1 g of Lu2O3, Eu2O3 and SiO2 raw material powders according to the stoichiometric ratio (the mass ratio of each raw material is Lu2O3:SiO2:Eu2O3=0.8315:0.1365:0.0320), and add 20 wt% of Na2CO3.
[0063] 2. Grind the above raw material mixture in an agate mortar for 30 to 60 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible, calcine it at 1300°C in air for 8 hours, then cool it to room temperature and grind it again for 30 to 60 minutes. Place it in an Al-reducing atmosphere and calcine it at 1200°C for 4 hours. Cool it to room temperature to obtain the target product.
[0064] 3. Use fluorescence spectrometer (HITACHI F-7500) to test the spectral properties of the phosphor in the system, such as Figure 1 As shown. The results show that the phosphor of this system has a wide excitation band, with a peak value near 370nm and a high spectral peak, which can match well with the commercial ultraviolet light chip. Under the excitation of 370nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (450-650nm) with a peak value at 504nm.
[0065] The ultraviolet excited Eu obtained in this example 2+ The general formula of doped green light emitting phosphor is Lu2SiO5:xEu 2+ , x is 0.04.
[0066] Example 5
[0067] This embodiment provides a method for preparing a purple light high-response green light phosphor for healthy lighting, the steps are:
[0068] 1. Weigh 1 g of Lu2O3, Eu2O3 and SiO2 raw material powders according to the stoichiometric ratio (the mass ratio of each raw material is Lu2O3:SiO2:Eu2O3=0.8218:0.1379:0.0404), and add 20 wt% of Na2CO3.
[0069] 2. Grind the above raw material mixture in an agate mortar for 30 to 60 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible, calcine it at 1200°C in air for 8 hours, then cool it to room temperature and grind it again for 30 to 60 minutes. Place it in an Al-reducing atmosphere and calcine it at 1100°C for 6 hours. Cool it to room temperature to obtain the target product.
[0070] 3. Use fluorescence spectrometer (HITACHI F-7500) to test the spectral properties of the phosphor in the system, such as Figure 1 As shown. The results show that the phosphor of this system has a wide excitation band, with a peak value near 370nm and a high spectral peak, which can match well with the commercial ultraviolet light chip. Under the excitation of 370nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (450-650nm) with a peak value at 504nm.
[0071] The ultraviolet excited Eu obtained in this example 2+ The general formula of doped green light emitting phosphor is Lu2SiO5:xEu 2+ , x is 0.05.
[0072] The raw material composition and process parameters of the preparation of the purple light high-response green light phosphors provided in the above different embodiments are specifically shown in Table 1.
[0073] Table 1 Preparation process parameters and performance test results of Examples 1-5
[0074] Example 1 2 3 4 5 <![CDATA[Lu2O3]]> 0.8621 0.8505 0.8411 0.8315 0.8218 <![CDATA[SiO2]]> 0.1302 0.1338 0.1351 0.1365 0.1379 <![CDATA[Eu2O3]]> 0.0078 0.0157 0.0237 0.0320 0.0404 <![CDATA[Na2CO3]]> 0.2 0.2 0.2 0.2 0.2 Sintering time (h) 8 8 6 8 8 Sintering temperature(℃) 1200 1250 1150 1300 1200 Restoration time (h) 6 6 4 4 6 Reduction temperature(℃) 1000 1050 1100 1200 1100 (Violet light) 400nm excitation maintains intensity 73% 75% 73.4% 75.5% 74%
[0075] The green light fluorescent material with high purple light response provided by the present invention is a new Eu 2+ The doped oxide-based 504nm blue light emitting fluorescent material has a wide excitation band, an effective absorption range covering 220-450nm, can be excited by ultraviolet and violet light, has the advantage of stable physical and chemical properties, and the luminous intensity is still maintained at more than 75% under 400nm excitation. It can be highly responsive to violet light excitation chips and can meet the urgent needs of current white light LEDs, sunlight-like LEDs, full-spectrum LEDs, and healthy lighting LED light sources.
[0076] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A green fluorescent material with high violet light response, characterized in that: The chemical expression of the fluorescent material is Lu2SiO5:xEu 2+ , where 0.01≤x≤0.
05.
2. The purple light highly responsive green light fluorescent material according to claim 1, characterized in that: The x=0.01, 0.02, 0.03, 0.04 or 0.
05.
3. The purple light highly responsive green light fluorescent material according to claim 1, characterized in that: The purple light high response green light fluorescent material is a powdery material.
4. The purple light highly responsive green light fluorescent material according to claim 1, characterized in that: The excitation spectrum range of the purple light high-response green light fluorescent material covers 200 to 470 nm, and the emission spectrum range covers 450 to 650 nm.
5. The purple light highly responsive green light fluorescent material according to claim 1, characterized in that: The emission intensity of the green fluorescent material with high violet light response maintains 75% of the optimal emission under the excitation of 400nm violet light.
6. A method for preparing the purple light highly responsive green light fluorescent material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) weighing raw material powders of a europium source compound, a lutetium source compound, and a silicon source compound according to a stoichiometric ratio, and grinding the raw material powders to uniformly mix them to obtain a mixture; (2) sintering the mixture obtained in step (1) at high temperature in air, and obtaining a powder after cooling; (3) Grinding the powder obtained in step (2) uniformly, then sintering it at high temperature by an Al reduction method, and obtaining the purple light high-response green light fluorescent material after cooling.
7. The method for preparing a purple light highly responsive green light fluorescent material according to claim 6, characterized in that: In step (1), after preparing various raw materials according to the chemical formula of the fluorescent material, 10-30 wt% Na2CO3 is added as a flux to reduce the reaction temperature.
8. The method for preparing a purple light highly responsive green light fluorescent material according to claim 6, characterized in that: In step (1), the europium source compound is Eu2O3, the lutetium source compound is Lu2O3, and the silicon source compound is SiO2.
9. The method for preparing a purple light highly responsive green light fluorescent material according to claim 6, characterized in that: The high temperature sintering conditions of step (2) are: sintering at 600-1400° C. for 1-10 hours; The high temperature sintering conditions of step (3) are as follows: mixing the ground powder with aluminum powder, and sintering at 500-1300° C. for 0.5-15 hours under vacuum conditions.
10. An application of the purple light high response green light fluorescent material according to any one of claims 1 to 5, characterized in that: The purple light high-response green light fluorescent material is used for healthy lighting.
Citation Information
Patent Citations
Green emitting phosphor and preparation method thereof
CN109609128A
Rare earth silicate phosphor and luminescent screen using the same
JP2002080847A
Cited By
Green fluorescent material excited by purple light as well as preparation method and application of green fluorescent material
CN119899666A
Purple light excitation type sunlight LED green light fluorescent powder and preparation method and application thereof
CN122344468A