Preparation method of mineral oil-based magnetorheological fluid

By activating and chemically coating carbonyl iron powder in dilute HCl, and combining it with the polycondensation reaction of nano-SiO2, a mineral oil-based magnetorheological fluid with high dispersion stability is prepared, which solves the problem of magnetorheological fluid dispersion stability and yield stress. problem, achieving long-term stability and performance improvements in vibration reduction and damping applications.

CN118725943AActive Publication Date: 2024-10-01ZIGONG ZHAOQIANG SEALING PROD IND +1

Patent Information

Application Number
CN202410767642.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing magnetorheological fluids have poor dispersion stability due to powder agglomeration and sedimentation after standing, and cannot meet long-term application requirements. The field-induced shear yield stress is high, which affects its performance in vibration reduction and damping applications.

Method used

By activating carbonyl iron powder in dilute HCl, using silane coupling agent and oleic acid for chemical coating, combined with the polycondensation reaction of nano-SiO2, a mineral oil-based magnetorheological fluid is prepared to achieve chemical coating of micron particles and nano Replacement of particles improves dispersion stability.

Benefits of technology

The prepared magnetorheological fluid has a sedimentation rate of less than 5% after standing for three months. It has high dispersion stability and reduces field-induced shear yield stress. It is suitable for vibration reduction, damping, military industry, aerospace and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725943A_ABST
    Figure CN118725943A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of mineral oil-based magnetorheological fluid, and relates to the technical field of preparation of damping and vibration attenuation materials, and the preparation method comprises the following steps: 1, activating carbonyl iron powder micron particles in diluted HCl; step 2, coating the carbonyl iron powder with a silane coupling agent in alcohol / water; step 3, carrying out ball-milling coating on the Fe / Co nano magnetic particles by using oleic acid; 4, the coated carbonyl iron powder, the coated Fe / Co particles and hydrophobic nano SiO2 are added into mineral oil according to a certain mass ratio, mechanical stirring is conducted, and the mineral oil-based magnetorheological fluid is prepared. After the high-dispersion-stability magnetorheological fluid prepared by the preparation method is stood for three months, the sedimentation rate is lower than 5%, and the high-dispersion-stability magnetorheological fluid has better dispersion stability and can be applied to the fields of vibration reduction, damping, military industry, aerospace and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of damping and vibration reduction materials, and in particular to a method for preparing a mineral oil-based magnetorheological fluid. Background Art

[0002] Magnetorheological fluid is a new type of smart material that can instantly transform from a liquid to a solid-like state under the influence of an external magnetic field. Traditional variable damping and microfluidic devices usually adjust damping or flow by controlling the number or size of channels, which often causes significant lag in their behavior. In order to overcome these limitations, the unique characteristics of magnetorheological fluid are utilized to replace hydraulic oil in traditional variable damping vibration reduction and microfluidic devices, which can effectively achieve these functions and conform to the current trend of intelligent development.

[0003] Magnetorheological fluid is usually composed of three parts: micron-sized magnetic powder, base carrier liquid and additives. Due to the large density difference between the magnetic powder and the base carrier liquid and the poor compatibility between the two, the magnetic powder is prone to agglomeration and sedimentation during use, which directly affects the rheological effect of the magnetorheological fluid and greatly reduces its application effect. This is also one of the key issues that need to be urgently solved in the current research on the preparation of magnetorheological fluids.

[0004] Patent CN1632891A adopts ball milling method to mix carbonyl iron powder particles, mineral oil, organic bentonite catalyst, surfactant and solid lubricant in a certain proportion and then ball mill them to prepare the magnetorheological fluid. Since it is difficult for the components to coat the particles through chemical reactions, the dispersion stability of the magnetorheological fluid cannot meet the long-term application requirements.

[0005] Patent CN107057810A, after heating poly-alpha olefin synthetic oil, add thixotropic agent organic bentonite, stir evenly; then add copolymer solution containing acidic groups as surfactant, stir evenly; then add anti-wear agent graphite, antioxidant sodium nitrite, stir evenly; then add carbonyl iron powder and disperse at high speed for 1 hour to obtain the finished magnetorheological fluid. Since the particle size is micron-level, it is difficult for surfactants to chemically coat the particles, so the dispersion stability of the prepared magnetorheological fluid cannot meet the needs of long-term application.

[0006] Patent CN114551022A, magnetic nanoparticles and thermosetting polymer materials (magnetic particles, composite accumulation magnetic nanoparticles, base carrier liquid, dispersant, anti-settling agent, lubricant, thixotropic agent, surfactant) are mixed and then heated and cured, and the solidified particles are broken, and then put into a ball mill equipped with a base carrier liquid for a long time. After the ball milling, the suspension is everywhere, and the large particles (composite accumulation magnetic nanoparticles) are repeatedly sucked away by magnets until the suspension does not separate solid and liquid, and finally the large particles are repeatedly washed with deionized water to obtain the required composite accumulation magnetic nanoparticles. Similarly, in the preparation process of this method, the surfactant and the particles are coated under heating, and it is difficult to achieve a stronger chemical coating. Therefore, when the solidified particles are difficult to be evenly dispersed in the base liquid after ball milling, it is difficult to prepare a magnetorheological fluid that can be dispersed and stabilized for a long time.

[0007] Patent CN113972061A uses an oxidation precipitation method to prepare Fe3O4 micron powder, chemically treats the powder surface, and then stirs it to cause strong chemical adsorption with carboxylic acids with multiple carboxyl functional groups. The coated powder is dispersed in a high-viscosity dispersing oil by stirring, ultrasound, and ball milling to prepare a magnetorheological fluid with high dispersion stability. The particles prepared by this invention patent have nanometer-scale particles. The smaller the particle size, the more conducive it is to stable dispersion in the base liquid. Therefore, no stratification occurs after centrifugation, and no stratification occurs after sedimentation for one month. The reduction in particle size will also have an adverse effect, that is, the magnetic properties of the particles will decrease, which will cause the prepared magnetorheological fluid to be under the shear yield stress under the magnetic field, which is not conducive to application.

[0008] It can be seen that the magnetorheological fluid prepared by simple mechanical mixing and physical action of magnetic powder, non-magnetic powder and various additives has a high sedimentation rate after standing for a period of time, and its dispersion stability cannot meet the application requirements of long-term shock absorption and damping of magnetorheological fluid. In addition, when improving the dispersion stability of magnetorheological fluid, the field-induced shear yield stress of magnetorheological fluid cannot be significantly reduced. Summary of the invention

[0009] Based on the problem of poor dispersion stability of the existing magnetorheological fluid caused by powder agglomeration and sedimentation in the background technology, the purpose of the present invention is to provide a method for preparing a mineral oil-based magnetorheological fluid with high dispersion stability. The magnetorheological fluid with high dispersion stability prepared by the preparation method has a sedimentation rate of less than 5% after standing for three months, has good dispersion stability, and can be used in vibration reduction, damping, military industry, aerospace and other fields.

[0010] The present invention is achieved through the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing a mineral oil-based magnetorheological fluid, comprising the following steps:

[0012] Step 1: Activating carbonyl iron powder micron particles in diluted HCl;

[0013] Step 2: Coating the carbonyl iron powder with a silane coupling agent in alcohol / water;

[0014] Step 3: ball milling and coating the Fe / Co nanomagnetic particles with surfactant oleic acid;

[0015] Step 4: Add coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 into mineral oil in a certain mass ratio, and stir mechanically to prepare a mineral oil-based magnetorheological fluid.

[0016] The principle of this technical solution is:

[0017] First, mineral oil is selected as the base carrier liquid. The surface of carbonyl iron powder is first activated by hydrochloric acid to attach a large number of -OH functional groups to its surface. Then, a silane coupling agent is used to chemically coat the particle surface in alcohol / water. Oleic acid is used to chemically coat nano Fe / Co particles under ball milling. Nano SiO2 is added in mineral oil to realize its own condensation reaction. Nano particles replace part of micro particles, which effectively improves the dispersion stability. The prepared mineral oil-based magnetorheological fluid has high dispersion stability.

[0018] As a better implementation method of the present application, the ratio of carbonyl iron powder to dilute hydrochloric acid added in step 1 is (10g~50g):(10ml~100ml); the dilute hydrochloric acid is diluted as follows: hydrochloric acid with a mass concentration of 36% is diluted with ultrapure water in a volume ratio of (10~20):(200~400).

[0019] Wherein, the stirring rate in step 1 is 600 rpm, the stirring time is 20 min, the temperature of the activation reaction is 40° C., and the particle size of the carbonyl iron powder is 1 to 5 μm.

[0020] As a preferred embodiment of the present application, in step 2, the carbonyl iron powder is coated with a silane coupling agent in alcohol / water, and the mass ratio of the silane coupling agent to the carbonyl iron powder is 1:(1-5).

[0021] Wherein, the coating time in step 2 is 1 to 3 hours, and the stirring rate is 300 to 500 r / min.

[0022] As a preferred embodiment of the present application, in step 2, the volume ratio of alcohol to water is (10-100): (50-400).

[0023] As a better implementation in the present application, in step 3, the mass ratio of oleic acid to Fe / Co nanomagnetic particles is (1-10):1.

[0024] The ball milling time in step 3 is 10 to 48 hours, and the steel balls used are 12.7 mm GCr19 standard steel balls.

[0025] As a preferred embodiment of the present application, the particle size distribution range of the nano-silicon dioxide added in step 4 is 50 nm to 500 nm.

[0026] As a better implementation method in the present application, the total mass proportion of the coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 in step 4 is 1% to 10%.

[0027] As a better implementation method in the present application, in terms of mass percentage, the coated carbonyl iron powder in step 4: coated Ee / Co particles: hydrophobic nano-SiO2 is (50%~95%): (1%~5%): (1%~10%).

[0028] As a preferred embodiment of the present application, the mechanical stirring rate in step 4 is 1000-2000 r / min, the time is 10-24 h, and the temperature is 50-80° C. The mass ratio of the total mass of the coated mixed powder to the mineral oil is 50%-80%.

[0029] In a second aspect, the present invention provides a mineral oil-based magnetorheological fluid prepared by any of the preparation methods described above.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] (1) The micron carbonyl iron powder and nano metal powder in the magnetorheological fluid prepared by the present invention are both chemically coated. Moreover, by using a portion of nano powder to replace the micron powder, the Brownian motion of the nano powder can be utilized. Therefore, the magnetorheological fluid prepared after dispersion has higher dispersion stability.

[0032] (2) The magnetorheological fluid prepared by the present invention also uses nano-silicon dioxide, which forms a network structure by its own polycondensation reaction in the solution, which can also promote the dispersion stability of the magnetorheological fluid;

[0033] (3) The magnetorheological fluid prepared by the present invention has a simple preparation process, a safe process, the required materials are easily available, and the equipment requirements are also very low. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0035] Figure 1 is a SEM image of the uncoated carbonyl iron powder described in Example 1 of the present invention;

[0036] Figure 2 This is a SEM image of the coated carbonyl iron powder described in Example 1 of the present invention;

[0037] Figure 3 The actual pictures of the magnetorheological fluid in Example 1 of the present invention before and after the application of a magnetic field, (a) without the application of a magnetic field, (b) under the application of a magnetic field;

[0038] Figure 4 This is a graph showing the dispersion stability of the magnetorheological fluids prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention after sedimentation for three months, and from left to right are samples of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0040] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] This embodiment provides a method for preparing a mineral oil-based magnetorheological fluid, which is carried out according to the following steps:

[0043] S1. Dilute hydrochloric acid with a mass concentration of 36% and ultrapure water in a volume ratio of 10 ml:300 ml, activate the carbonyl iron powder micron particles in the diluted HCl, and add carbonyl iron powder and diluted hydrochloric acid in a ratio of 20g:80ml. In addition, the stirring rate is 600rpm, the stirring time is 20min, the activation reaction temperature is 40°C, and the particle size of the carbonyl iron powder is 1-5μm.

[0044] S2. The carbonyl iron powder was coated with a silane coupling agent (dodecyltrimethoxysilane) in alcohol / water. The mass ratio of dodecyltrimethoxysilane to carbonyl iron powder was 1:4, the volume ratio of alcohol: water was 20 ml: 300 ml, the coating time was 2 hours, and the stirring rate was 300 r / min.

[0045] S3. The Fe / Co nanomagnetic particles were coated by ball milling using oleic acid. The mass ratio of oleic acid to Fe / Co nanomagnetic particles was 1:1. The ball milling time was 24 hours. The steel ball used was a 12.7 mm GCr19 standard steel ball.

[0046] S4. Add carbonyl iron powder: SiO2: Fe / Co into mineral oil in a ratio of 90%:5%:5%, wherein the total mass of coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 accounts for 5%, wherein the particle size distribution range of nano-silicon dioxide is 50nm~500nm, and prepare a magnetorheological fluid with high dispersion stability by mechanical stirring, wherein the mechanical stirring rate is 1000r / min, the time is 10 hours, the temperature is 70°C, and the mass ratio of the total mass of the coated mixed powder to the mineral oil is 70%.

[0047] After the magnetorheological fluid prepared in Example 1 was left to stand for three months, the sedimentation rate was 4%. Figure 4 As shown, it shows that the prepared magnetorheological fluid has high dispersion stability.

[0048] like Figure 1 , which is a SEM image of the uncoated carbonyl iron powder in Example 1; it can be seen from the image that the surface of the uncoated carbonyl iron powder particles is smooth, and there is no obvious agglomeration between the particles.

[0049] like Figure 2 As shown, it is a SEM image of the coated carbonyl iron powder in Example 1; it can be seen from the figure that obvious floccules appear on the surface of the coated carbonyl iron powder particles, and some particles are agglomerated, which is caused by the adhesion between the particles due to the action of the surfactant. Figure 1 and Figure 2 The comparison shows that the active agent is effectively coated on the surface of the particles.

[0050] like Figure 3The following are the actual pictures of the magnetorheological fluid in Example 1 before and after the application of a magnetic field, (a) without the application of a magnetic field, and (b) under a magnetic field. As can be seen from Figure (a), when no magnetic field is applied, the magnetorheological fluid is in a black flowing state, which is no different from a conventional black colloid; after the application of a magnetic field, a spike structure instantly bulges on the surface of the magnetorheological fluid, and the fluidity becomes poor, approaching a semi-solid structure. Before and after the application of a magnetic field, the magnetorheological fluid undergoes a transformation from a liquid state to a quasi-solid state, and it is precisely by utilizing the difference in its rheological properties that the vibration problem of the main shaft of the turbine is effectively solved.

[0051] Example 2

[0052] This embodiment provides a method for preparing a mineral oil-based magnetorheological fluid, which is carried out according to the following steps:

[0053] S1. Dilute hydrochloric acid with a mass concentration of 36% and ultrapure water in a volume ratio of 20 ml:400 ml, activate the carbonyl iron powder micron particles in the diluted hydrochloric acid, and add carbonyl iron powder and diluted hydrochloric acid in a ratio of 40g:50ml. In addition, the stirring rate is 600rpm, the stirring time is 20min, the activation reaction temperature is 40°C, and the particle size of the carbonyl iron powder is 1-5μm.

[0054] S2. The carbonyl iron powder was coated with a silane coupling agent (dodecyltrimethoxysilane) in alcohol / water. The mass ratio of dodecyltrimethoxysilane to carbonyl iron powder was 1:3, the volume ratio of alcohol: water was 20 ml: 400 ml, the coating time was 3 hours, and the stirring rate was 400 r / min.

[0055] S3. The Fe / Co nanomagnetic particles were coated by ball milling using oleic acid. The mass ratio of oleic acid to Fe / Co nanomagnetic particles was 3:1. The ball milling time was 48 hours. The steel ball used was a 12.7 mm GCr19 standard steel ball.

[0056] S4. Add carbonyl iron powder: SiO2: Fe / Co into mineral oil in a ratio of 85%: 5%: 10%, wherein the total mass of coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 accounts for 1%, and the particle size distribution range of nano-silicon dioxide is 50nm~500nm, to prepare a magnetorheological fluid with high dispersion stability, wherein the mechanical stirring rate is 2000r / min, the time is 24 hours, the temperature is 80°C, and the mass ratio of the total mass of the coated mixed powder to the mineral oil is 80%.

[0057] After the magnetorheological fluid prepared in Example 2 was left to stand for three months, the sedimentation rate was 4.5%, indicating that the magnetorheological fluid prepared had high dispersion stability.

[0058] Example 3

[0059] This embodiment provides a method for preparing a mineral oil-based magnetorheological fluid, which is carried out according to the following steps:

[0060] S1. Dilute hydrochloric acid with a mass concentration of 36% and ultrapure water in a volume ratio of 15 ml:300 ml, activate the carbonyl iron powder micron particles in the diluted HCl, and add carbonyl iron powder and diluted hydrochloric acid in a ratio of 50g:100ml. In addition, the stirring rate is 600rpm, the stirring time is 20min, the activation reaction temperature is 40°C, and the particle size of the carbonyl iron powder is 1-5μm.

[0061] S2. The carbonyl iron powder was coated with a silane coupling agent (dodecyltrimethoxysilane) in alcohol / water. The mass ratio of dodecyltrimethoxysilane to carbonyl iron powder was 1:1, the volume ratio of alcohol: water was 12 ml: 300 ml, the coating time was 2 hours, and the stirring rate was 300 r / min.

[0062] S3. The Fe / Co nanomagnetic particles were coated by ball milling using oleic acid. The mass ratio of oleic acid to Fe / Co nanomagnetic particles was 5:1. The ball milling time was 25 hours. The steel ball used was a 12.7 mm GCr19 standard steel ball.

[0063] S4. Add carbonyl iron powder: SiO2: Fe / Co into mineral oil in a ratio of 50%: 1%: 10%, wherein the total mass of coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 accounts for 10%, and the particle size distribution range of nano-silicon dioxide is 50nm~500nm. Mechanical stirring is carried out to prepare a magnetorheological fluid with high dispersion stability, wherein the mechanical stirring rate is 1500r / min, the time is 10 hours, the temperature is 50°C, and the mass ratio of the total mass of the coated mixed powder to the mineral oil is 50%.

[0064] After the magnetorheological fluid prepared in Example 3 was left to stand for three months, the sedimentation rate was 5%. Figure 4 As shown, it shows that the prepared magnetorheological fluid has high dispersion stability.

[0065] Example 4

[0066] This embodiment provides a method for preparing a mineral oil-based magnetorheological fluid, which is different from that of embodiment 1 in that the ratio of carbonyl iron powder to dilute hydrochloric acid in step S1 of this embodiment is 10 g:10 ml. Other steps and process conditions are the same as those of embodiment 1.

[0067] Follow these steps:

[0068] S1. Dilute hydrochloric acid with a mass concentration of 36% and ultrapure water in a volume ratio of 10 ml:300 ml, activate the carbonyl iron powder micron particles in the diluted HCl, and add carbonyl iron powder and diluted hydrochloric acid in a ratio of 10g:10ml. In addition, the stirring rate is 600rpm, the stirring time is 20min, the activation reaction temperature is 40°C, and the particle size of the carbonyl iron powder is 1-5μm.

[0069] S2. The carbonyl iron powder was coated with a silane coupling agent (dodecyltrimethoxysilane) in alcohol / water. The mass ratio of dodecyltrimethoxysilane to carbonyl iron powder was 1:4, the volume ratio of alcohol: water was 20 ml: 300 ml, the coating time was 2 hours, and the stirring rate was 300 r / min.

[0070] S3. The Fe / Co nanomagnetic particles were coated by ball milling using oleic acid. The mass ratio of oleic acid to Fe / Co nanomagnetic particles was 10:1. The ball milling time was 24 hours. The steel ball used was a 12.7 mm GCr19 standard steel ball.

[0071] S4. Add carbonyl iron powder: SiO2: Fe / Co into mineral oil in a ratio of 90%:5%:5%, wherein the total mass of coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 accounts for 5%, wherein the particle size distribution range of nano-silicon dioxide is 50nm~500nm, and prepare a magnetorheological fluid with high dispersion stability by mechanical stirring, wherein the mechanical stirring rate is 1000r / min, the time is 10 hours, the temperature is 70°C, and the mass ratio of the total mass of the coated mixed powder to the mineral oil is 70%.

[0072] It was determined that after the magnetorheological fluid prepared in this embodiment was left to stand for three months, the sedimentation rate was the same as that in Example 1, which was 4%, indicating that the magnetorheological fluid prepared had high dispersion stability.

[0073] Example 5

[0074] This embodiment provides a method for preparing a mineral oil-based magnetorheological fluid. The difference from Embodiment 1 is that in step 2 of this embodiment, the mass ratio of the silane coupling agent to the carbonyl iron powder is 1:5, and the other steps and process conditions are the same as those of Embodiment 1. The following steps are performed:

[0075] S1. Dilute hydrochloric acid with a mass concentration of 36% and ultrapure water in a volume ratio of 10 ml:300 ml, activate the carbonyl iron powder micron particles in the diluted HCl, and add carbonyl iron powder and diluted hydrochloric acid in a ratio of 20g:80ml. In addition, the stirring rate is 600rpm, the stirring time is 20min, the activation reaction temperature is 40°C, and the particle size of the carbonyl iron powder is 1-5μm.

[0076] S2. The carbonyl iron powder was coated with a silane coupling agent (dodecyltrimethoxysilane) in alcohol / water. The mass ratio of dodecyltrimethoxysilane to carbonyl iron powder was 1:5, the volume ratio of alcohol: water was 20 ml:300 ml, the coating time was 2 hours, and the stirring rate was 300 r / min.

[0077] S3. Fe / Co nanomagnetic particles were coated by ball milling using oleic acid. The mass ratio of oleic acid to Fe / Co nanomagnetic particles was 8:1. The ball milling time was 24 hours. The steel ball used was a 12.7 mm GCr19 standard steel ball.

[0078] S4. Add carbonyl iron powder: SiO2: Fe / Co into mineral oil in a ratio of 90%:5%:5%, wherein the total mass of coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 accounts for 5%, wherein the particle size distribution range of nano-silicon dioxide is 50nm~500nm, and prepare a magnetorheological fluid with high dispersion stability by mechanical stirring, wherein the mechanical stirring rate is 1000r / min, the time is 10 hours, the temperature is 70°C, and the mass ratio of the total mass of the coated mixed powder to the mineral oil is 70%.

[0079] It was determined that after the magnetorheological fluid prepared in this embodiment was left to stand for three months, the sedimentation rate was the same as that in Example 2, which was 4.5%, indicating that the magnetorheological fluid prepared in this embodiment had high dispersion stability.

[0080] Example 6

[0081] This embodiment provides a method for preparing a mineral oil-based magnetorheological fluid. The difference from Example 1 is that the mass ratio of oleic acid to Fe / Co nanomagnetic particles in this embodiment is 1:10, and the other steps and process conditions are the same as those in Example 1. The following steps are performed:

[0082] S1. Dilute hydrochloric acid with a mass concentration of 36% and ultrapure water in a volume ratio of 10 ml:300 ml, activate the carbonyl iron powder micron particles in the diluted HCl, and add carbonyl iron powder and diluted hydrochloric acid in a ratio of 20g:80ml. In addition, the stirring rate is 600rpm, the stirring time is 20min, the activation reaction temperature is 40°C, and the particle size of the carbonyl iron powder is 1-5μm.

[0083] S2. The carbonyl iron powder was coated with a silane coupling agent (dodecyltrimethoxysilane) in alcohol / water. The mass ratio of dodecyltrimethoxysilane to carbonyl iron powder was 1:4, the volume ratio of alcohol: water was 20 ml: 300 ml, the coating time was 2 hours, and the stirring rate was 300 r / min.

[0084] S3. The Fe / Co nanomagnetic particles were coated by ball milling using oleic acid. The mass ratio of oleic acid to Fe / Co nanomagnetic particles was 6:1. The ball milling time was 24 hours. The steel ball used was a 12.7 mm GCr19 standard steel ball.

[0085] S4. Add carbonyl iron powder: SiO2: Fe / Co into mineral oil in a ratio of 90%:5%:5%, wherein the total mass of coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 accounts for 5%, wherein the particle size distribution range of nano-silicon dioxide is 50nm~500nm, and prepare a magnetorheological fluid with high dispersion stability by mechanical stirring, wherein the mechanical stirring rate is 1000r / min, the time is 10 hours, the temperature is 70°C, and the mass ratio of the total mass of the coated mixed powder to the mineral oil is 70%.

[0086] It was determined that after the magnetorheological fluid prepared in this embodiment was left to stand for three months, the sedimentation rate was the same as that in Example 3, which was 5%, indicating that the magnetorheological fluid prepared had high dispersion stability.

[0087] Comparative Example 1

[0088] This comparative example provides a method for preparing a magnetorheological fluid. The specific preparation method is basically the same as that of Example 1. The difference between the two is that hydrochloric acid is not used to corrode the particles in step S1, and the conditions of the remaining steps are the same as those of Example 1.

[0089] The magnetorheological fluid prepared in Comparative Example 1 was left to stand for three months, and the sedimentation rate was as high as 22%. Figure 4 As shown, it is shown that the dispersion stability of the prepared magnetorheological fluid is very poor.

[0090] Comparative Example 2

[0091] This comparative example provides a method for preparing a magnetorheological fluid. The specific preparation method is basically the same as that of Example 1. The difference between the two is that ethanol is not used in step S2, and the conditions of the other steps are the same as those of Example 1.

[0092] The magnetorheological fluid prepared in Comparative Example 2 was left to stand for three months, and the sedimentation rate was as high as 20%. Figure 4 As shown, it is shown that the dispersion stability of the prepared magnetorheological fluid is very poor.

[0093] Comparative Example 3

[0094] This comparative example provides a method for preparing a magnetorheological fluid. The specific preparation method is basically the same as that of Example 1. The difference between the two is that oleic acid is not used for coating in step S3, and the conditions of the other steps are the same as those of Example 1.

[0095] The magnetorheological fluid prepared in Comparative Example 3 was left to stand for three months, and the sedimentation rate was as high as 18%. Figure 4 As shown, it is shown that the dispersion stability of the prepared magnetorheological fluid is very poor.

[0096] Comparative Example 4

[0097] This comparative example provides a method for preparing a magnetorheological fluid. The specific preparation method is basically the same as that of Example 1. The difference between the two is that SiO2 is not added in step S4, and the conditions of the remaining steps are the same as those of Example 1.

[0098] The magnetorheological fluid prepared in Comparative Example 4 was left to stand for three months, and the sedimentation rate was as high as 21%. Figure 4 As shown, it is shown that the dispersion stability of the prepared magnetorheological fluid is very poor.

[0099] from Figure 4 It can be seen from the sedimentation results of the embodiments and comparative examples that, when reacted under different conditions, the dispersion stability of the prepared magnetorheological fluid after sedimentation for three months showed obvious differences. Only by preparing according to the preparation method and process conditions in this application can a magnetorheological fluid with high dispersion stability be obtained, which not only improves the dispersion stability of the magnetorheological fluid, but also has a higher field-induced shear yield stress.

[0100] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a mineral oil-based magnetorheological fluid, characterized in that: The following steps are involved: Step 1: Activating carbonyl iron powder micron particles in diluted HCl; Step 2: Coating the carbonyl iron powder with a silane coupling agent in alcohol / water; Step 3: ball milling and coating the Fe / Co nanomagnetic particles with surfactant oleic acid; Step 4: Add coated carbonyl iron powder, coated Fe / Co particles and hydrophobic nano-SiO2 into mineral oil in a certain mass ratio, and stir mechanically to prepare a mineral oil-based magnetorheological fluid.

2. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: The amount ratio of the carbonyl iron powder and the dilute hydrochloric acid added in step 1 is (10g-50g):(10ml-100ml); wherein the dilute hydrochloric acid is diluted as follows: hydrochloric acid with a mass concentration of 36% is diluted with ultrapure water in a volume ratio of (10-20):(200-400).

3. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: In step 2, the carbonyl iron powder is coated with a silane coupling agent in alcohol / water, and the mass ratio of the silane coupling agent to the carbonyl iron powder is 1:(1-5).

4. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: In step 2, the volume ratio of alcohol to water is (10-100):(50-400).

5. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: In step 3, the mass ratio of surfactant oleic acid to Fe / Co nanomagnetic particles is (1-10):

1.

6. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: The particle size distribution range of the nano silicon dioxide added in step 4 is 50nm to 500nm.

7. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: In step 4, the total mass proportion of the coated carbonyl iron powder, the coated Fe / Co particles and the hydrophobic nano-SiO2 is 1% to 10%.

8. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: In terms of mass percentage, the coated carbonyl iron powder in step 4: coated Ee / Co particles: hydrophobic nano-SiO2 are (50% to 95%): (1% to 5%): (1% to 10%).

9. The method for preparing a mineral oil-based magnetorheological fluid according to claim 1, characterized in that: The mechanical stirring rate in step 4 is 1000-2000 r / min, the time is 10-24 h, and the temperature is 50-80° C.

10. A mineral oil-based magnetorheological fluid, characterized in that: The preparation method is described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Mineral oil based magnetorheological fluid for high power transmission and preparation method thereof

    CN104560301A

  • Preparation method of magnetorheological fluid with high dispersion stability

    CN113972061A

  • Preparation method of synthetic oil-based magnetorheological fluid with high dispersion stability

    CN116387007A

  • A method for praparing Magnetorheological Fluid

    KR1020130104066A

Cited By

  • Preparation method of zero-valent iron reduction material with micro-nano size and water stability

    CN119566321A