Accurate grouting cooling method for high-temperature carbon bricks of blast furnace hearth
By opening grouting holes at high temperature points, the carbon grouting material is used to achieve precise cooling of the carbon bricks in the blast furnace hearth, solving the erosion problem caused by the high temperature of the carbon bricks in the hearth, extending the life of the blast furnace and improving safety and cooling efficiency.
Patent Information
- Application Number
- CN202410927307.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
AI Technical Summary
The high temperature of the carbon bricks in the blast furnace hearth leads to increased corrosion. The existing grouting method cannot achieve precise cooling due to the limited position and insufficient number of openings, resulting in poor heat conduction in the hearth, shortening the life of the blast furnace, and even causing burn-through accidents.
Open holes for grouting at high temperature points, use carbonaceous grouting material to perform precise grouting at the gap between the cooling wall and the carbon brick, control the pressure and temperature of the grouting material to ensure its uniform distribution and solidification, and create circular holes with a diameter of 5-10cm , the filler is silica sand or graphite powder and refractory binder.
It achieves precise cooling of carbon bricks, extends the life of the blast furnace, reduces the number of openings, improves safety and cooling efficiency, ensures heat conduction, and avoids burn-through accidents.
Smart Images

Figure CN118726671A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of blast furnaces in the metallurgical industry, and in particular relates to a precise grouting and cooling method for high-temperature carbon bricks in a blast furnace hearth. Background Art
[0002] With the development of blast furnace oxygen enrichment technology, blast furnace output has increased, and the amount of slag and iron passing through the unit cross-sectional area of the furnace per unit time has increased significantly, causing erosion of the carbon bricks in the furnace. When the blast furnace is shut down and resumed, the gap between the carbon bricks and the cooling wall increases due to thermal expansion and contraction, and water or gas may enter the gap to form a channel. The thermal conductivity of water or gas is lower than that of the filling material between the carbon bricks and the cooling wall, resulting in the carbon bricks in contact with the slag and iron being unable to dissipate heat in time after being heated, aggravating the erosion of the carbon bricks and causing the carbon bricks to have a high temperature.
[0003] The existing method of driving out water or gas is generally to grout the furnace, and the opening position during grouting is generally selected in the gap between the two cooling walls. At present, each blast furnace is equipped with a furnace erosion diagnosis system, and the temperature measuring couples used are distributed in large numbers between the gaps of the furnace cooling walls, resulting in the lack of suitable opening positions for grouting in some high-temperature areas of the side walls, or the actual high-temperature points are very likely not in the gap between the cooling wall and the carbon bricks. Therefore, the limitation of the opening position results in poor effect of sealing the gaps after grouting. As a result, the temperature of the side walls of the furnace is high for a long time, and the heat in the furnace cannot be conducted out, which leads to abnormal erosion of the carbon bricks in the furnace, shortening the life of the blast furnace, and causing serious accidents such as furnace burn-through in severe cases. At present, each blast furnace mainly increases the number of openings during the wind stop, trying to solve the probability problem of sealing the gaps by quantity, but cannot achieve precise grouting. Summary of the invention
[0004] The purpose of the present invention is to provide a precise grouting and cooling method for high-temperature carbon bricks in the hearth of a blast furnace, which changes the previous method of grouting by opening holes in the gaps of the cooling wall to grouting by opening holes on the cooling wall where the high-temperature points are located, thereby solving the limitations of the distribution monitoring of multiple detection couples in the hearth and the location of the holes in the high-temperature zone, and realizes rapid and precise hole opening. Precise grouting can achieve a rapid drop in the side wall temperature, thereby improving the safety and cooling efficiency of the blast furnace.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a precise grouting cooling method for high-temperature carbon bricks in a blast furnace hearth, comprising the following steps:
[0006] 1) Determine the cooling wall where the carbon brick temperature is high;
[0007] 2) Drill a hole on the determined cooling wall, and the hole depth reaches the gap between the cooling wall and the carbon brick;
[0008] 3) Inject carbon grouting material into the hole to achieve precise grouting at a fixed point;
[0009] 4) Control the grouting pressure and temperature to ensure that the carbonaceous grouting material is evenly distributed and solidified in the furnace cooling wall.
[0010] Specifically, the opening is a circular hole with a diameter of 5 to 10 cm.
[0011] Specifically, the opening directly penetrates the cooling wall in the furnace area.
[0012] Specifically, the carbonaceous grouting material comprises filler, graphite powder and refractory binder, wherein the filler is silica sand or other high temperature resistant non-metallic minerals.
[0013] The present invention has the following beneficial effects:
[0014] 1) The carbon bricks in the furnace area are accurately cooled and the service life of the carbon bricks is extended;
[0015] 2) Reduce the number of openings in the blast furnace hearth area and improve safety;
[0016] 3) After grouting, drive away the moisture or gaps between the cooling wall and the carbon bricks, restore heat transfer, and improve cooling efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a diagram of the hole locations and depths of the blast furnace hearth.
[0018] In the figure: 1-carbon grouting material; 2-hole; 3-furnace shell; 4-carbon brick; 5-cooling wall. DETAILED DESCRIPTION
[0019] The present invention will now be described in further detail with reference to the accompanying drawings.
[0020] like Figure 1 As shown, a precise grouting cooling method for high temperature carbon bricks in a blast furnace hearth comprises the following steps:
[0021] 1) Determine the cooling wall 5 where the high temperature point of the carbon brick 4 is located;
[0022] 2) Drilling a hole on the determined cooling wall 5, the drilling depth reaches the gap between the cooling wall 5 and the carbon brick 4, the diameter of the hole is a circular hole 2 of 5 to 10 cm, and the hole is drilled directly through the cooling wall 5 in the furnace area;
[0023] 3) injecting the carbonaceous grouting material 1 into the hole 2 to achieve precise grouting at a fixed point;
[0024] 4) Controlling the grouting pressure and temperature to ensure that the carbonaceous grouting material 1 is evenly distributed and solidified in the furnace cooling wall 5.
[0025] The carbonaceous grouting material 1 comprises filler, graphite powder and refractory binder, wherein the filler is silica sand or other high temperature resistant non-metallic minerals.
[0026] Embodiment 1:
[0027] A precise grouting cooling method for high-temperature carbon bricks in a blast furnace hearth, comprising the following steps:
[0028] 1) using a hole-opening device to open a circular hole 2 with a diameter of 8 cm in the middle of the blast furnace hearth cooling wall 5, and the length of the hole 2 is 30 cm;
[0029] 2) preparing a carbon grouting material 1, wherein graphite powder accounts for 65%, a refractory binder accounts for 15%, and a silica sand filler accounts for 20%;
[0030] 3) injecting the carbonaceous grouting material 1 into the hole 2 using a grouting device, and using a temperature monitoring system and a pressure control system to ensure uniform distribution and proper solidification of the grouting material in the cooling wall;
[0031] 4) After grouting is completed, use temperature sensors to monitor the temperature distribution of the cooling wall to ensure that the cooling effect achieves the expected goal.
[0032] Embodiment 2:
[0033] A precise grouting cooling method for high-temperature carbon bricks in a blast furnace hearth, comprising the following steps:
[0034] 1) The same hole-opening method as in Example 1 was used, but the diameter of all holes 2 was adjusted to 10 cm to increase the grouting area;
[0035] 2) adjusting the proportion of carbonaceous grouting material 1, graphite powder accounts for 70%, refractory binder accounts for 10%, silica sand filler accounts for 20%, and adding a small amount of high temperature additives to improve the stability and temperature resistance of the grouting material;
[0036] 3) Use improved grouting equipment and pressure control systems to accurately control the injection volume and pressure of grouting materials to optimize the curing process and cooling effect;
[0037] 4) After the grouting is completed, the temperature of the cooling wall 5 is monitored for a long time to analyze the durability and cooling effect of the grouting material to optimize subsequent operations.
[0038] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0039] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A precise grouting cooling method for high temperature carbon bricks in blast furnace, characterized in that: The following steps are involved: 1) Determine the cooling wall where the carbon brick temperature is high; 2) Drill a hole on the determined cooling wall, and the hole depth reaches the gap between the cooling wall and the carbon brick; 3) Inject carbon grouting material into the hole to achieve precise grouting at a fixed point; 4) Control the grouting pressure and temperature to ensure that the carbonaceous grouting material is evenly distributed and solidified in the furnace cooling wall.
2. According to claim 1, a precise grouting cooling method for high-temperature carbon bricks in a blast furnace hearth is characterized in that: The opening has a diameter of 5 to 10 cm.
3. The precise grouting cooling method for high-temperature carbon bricks in a blast furnace according to claim 1 is characterized in that: The opening directly penetrates the cooling wall of the furnace area.
4. The method for precise grouting and cooling of high-temperature carbon bricks in a blast furnace according to claim 1, characterized in that: The carbonaceous grouting material comprises filler, graphite powder and refractory binder, wherein the filler is silica sand or other high temperature resistant non-metallic minerals.
Citation Information
Cited By
Blast furnace hearth grouting method, system, equipment and medium
CN120989317A