Vanadium titano-magnetite smelting process

Through the electric furnace secondary melting process, the problem of iron loss and difficulty in slag-iron separation caused by high titanium in vanadium-titanium magnetite is solved, and efficient iron, titanium, and vanadium recovery and energy consumption reduction are achieved.

CN118726685APending Publication Date: 2024-10-01SHANGHAI MILESTONE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410890126.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The high titanium content in vanadium-titanium magnetite leads to the formation of low-priced titanium in the slag, which increases the surface tension of the small iron beads, leading to iron loss and difficulty in slag-iron separation.

Method used

The electric furnace secondary melting process is used to recover iron, titanium and vanadium respectively through the steps of grinding, rotary kiln coal base reduction, electric furnace primary melting, high-temperature granulation of liquid vanadium-containing titanium slag and electric furnace secondary melting reduction, reducing the Iron loss and avoid difficulty in slag-iron separation.

Benefits of technology

It effectively reduces the iron loss by 6%-8%, avoids the difficulty of slag and iron separation, simplifies the process operation, and reduces energy consumption through the waste heat supplementation of the high-temperature granulation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004927232450000011
    Figure HDA0004927232450000011
Patent Text Reader

Abstract

The invention discloses a vanadium titano-magnetite smelting process, and belongs to the technical field of pyrometallurgy. According to the method, secondary melting separation is conducted through the electric furnace, iron, titanium and vanadium are recycled, iron loss is reduced, meanwhile, the phenomenon that slag and iron are difficult to separate is avoided, iron loss with the weight ratio of 6%-8% is avoided, the phenomenon that slag and iron are difficult to separate does not exist, technological operation treatment is simple, and meanwhile energy consumption in the production process is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pyrometallurgy, and in particular relates to a vanadium-titanium magnetite smelting process. Background Art

[0002] At present, vanadium-titanium magnetite is mainly smelted in blast furnaces. The blast furnace smelting method usually includes: sintering vanadium-titanium iron concentrate and ordinary powder ore to produce sintered ore, using vanadium-titanium iron concentrate and ordinary iron concentrate to produce pelletized ore, and then adding the sintered ore, pelletized ore and a small amount of lump ore into the blast furnace together with coke in a certain proportion, and at the same time injecting coal powder and blowing air through the blast furnace tuyere to burn the coke and the injected coal powder to generate reducing gas (mainly CO and H 2 ), the reducing gas removes oxygen from the vanadium-titanium magnetite during its rise in the furnace, reducing it to obtain iron, which then melts and drips into the furnace to separate the slag and iron, thus completing the smelting process.

[0003] However, the titanium content in vanadium-titanium magnetite is relatively high, which makes TiO 2 The content is high, while TiO 2 Over-reduction will generate low-valent titanium with high melting points (such as TiC, TiN and TiCN). These low-valent titanium are adsorbed on the small iron beads, which increases the surface tension of the small iron beads, making it difficult for them to aggregate and grow, resulting in a large number of dispersed small iron beads in the slag. Moreover, the higher the content of the low-valent titanium in the slag, the more corresponding high-melting-point minerals there are, causing the slag melting temperature to rise, the slag viscosity to increase, and the slag-iron separation to be difficult. These factors lead to a high iron content in the slag produced during the smelting process of vanadium-titanium magnetite blast furnace, resulting in a large amount of iron loss, usually as high as 6%-8% by weight. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a vanadium-titanium magnetite smelting process, which adopts secondary smelting in an electric furnace to recover iron, titanium and vanadium respectively, thereby reducing iron loss and avoiding the difficulty in separating slag from iron.

[0005] In order to achieve the above object, the present invention provides a vanadium-titanium magnetite smelting process, which specifically comprises the following steps:

[0006] Step 1: Grinding of vanadium-titanium magnetite

[0007] The vanadium-titanium magnetite ore is crushed and ground, and the grinding particle size is required to be below 200 mesh, accounting for more than 80%; the iron content of the vanadium-titanium magnetite ore is 30%-50%, and the vanadium content is 0.2%-1.5%;

[0008] Step 2: Coal-based reduction in rotary kiln

[0009] The crushed vanadium-titanium magnetite is added with 30%-40% coal powder by weight and put into the rotary kiln. The mixed material is roasted in the rotary kiln for 1h-2h at a roasting temperature of 800℃-900℃.

[0010] Step 3: Electric furnace primary melting

[0011] The roasted and reduced vanadium-titanium magnetite is transported to an electric furnace, and the electrodes of the electric furnace convert electrical energy into heat energy to melt the vanadium-titanium magnetite. The electric furnace smelts for 4h-6h per furnace at a smelting temperature of 1200℃-1400℃. The vanadium-titanium magnetite is melted once to form molten steel and liquid vanadium-titanium slag. The molten steel is cooled to form steel products, and the liquid vanadium-titanium slag enters the next system; the iron content in the molten steel is greater than 95%;

[0012] Step 4: High temperature granulation of liquid vanadium-titanium slag

[0013] After the liquid vanadium-titanium slag is transported to the high-temperature granulator, 8%-10% by weight of petroleum coke and 15%-20% by weight of titanium ore with a grade of 46 or above are added, and after being mixed with the high-temperature liquid vanadium-titanium slag, it is transformed into high-temperature solid spherical particles through the high-temperature granulator, and the particle diameter is 10mm-15mm. The high-temperature granulator here can recycle heat energy and transport it to the rotary kiln for supplementary heat for coal-based reduction; wherein, the temperature of the high-temperature liquid vanadium-titanium slag is 1000℃-1200℃; the temperature of the high-temperature granulator is 80℃0-900℃; the temperature of the high-temperature solid spherical particles is guaranteed to be 500℃-600℃;

[0014] Step 5: Secondary melting reduction in electric furnace

[0015] The high-temperature granulated particles enter the insulation tank for insulation, and then are transferred to the electric furnace for secondary melting reduction; wherein, the insulation temperature is 500℃~600℃; the electric furnace smelts for 3h-4h per furnace, and the smelting temperature is 1000℃-1200℃. The vanadium-titanium magnetite is smelted to form high-titanium slag and liquid high-vanadium pig iron after secondary melting. The high-titanium slag can be sold after cooling, and the liquid high-vanadium pig iron enters the next system; wherein, the vanadium content in the liquid high-vanadium pig iron is 6%~8%;

[0016] Step 6: Converter Blowing

[0017] Liquid high-vanadium pig iron is blown in a converter to form semi-steel and vanadium slag. The blowing temperature is 1200℃-1250℃ and the blowing time is 50min-60min. Among them, the iron content in the semi-steel is higher than 95%, and the V content in the vanadium slag is 2 O 5 Content higher than 16%;

[0018] Compared with the existing process, the beneficial effects of the present invention are:

[0019] (1) The present invention performs secondary melting of vanadium-titanium magnetite, thereby avoiding the iron loss of 6%-8% by weight;

[0020] (2) The present invention does not have the problem of difficulty in separating slag and iron, and the process operation is simple;

[0021] (3) The waste heat from the high-temperature granulation process of the present invention can be used to supplement the heat for coal-based reduction, thereby reducing energy consumption in the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a process flow chart of a vanadium-titanium magnetite smelting process. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments. Figure 1 shown.

[0024] Example 1

[0025] A vanadium-titanium magnetite smelting process specifically comprises the following steps:

[0026] Step 1: Grinding of vanadium-titanium magnetite

[0027] The vanadium-titanium magnetite ore is crushed and ground, and the grinding particle size is required to be below 200 mesh, accounting for 80%. The composition of the vanadium-titanium magnetite is shown in Table 1:

[0028] Table 1. Element composition of vanadium-titanium magnetite ore (%)

[0029] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 48.03 0.37 22.31 1.52 3.15 0.011 0.015 0.043 0.84

[0030] Step 2: Coal-based reduction in rotary kiln

[0031] The crushed vanadium-titanium magnetite is added with 30% coal powder by weight and put into the rotary kiln. The mixed material is roasted in the rotary kiln for 1 hour at a roasting temperature of 800°C.

[0032] Step 3: Electric furnace primary melting

[0033] The roasted and reduced vanadium-titanium magnetite is transported to the electric furnace. The three electrodes of the electric furnace convert the electrical energy into heat energy to melt the vanadium-titanium magnetite. The electric furnace smelts for 6 hours per furnace, and the smelting temperature is 1400℃. The vanadium-titanium magnetite is melted once to form molten steel and liquid vanadium-titanium slag. The molten steel is cooled to form steel products, and the liquid vanadium-titanium slag enters the next system. The components of the liquid vanadium-titanium slag and molten steel are shown in Tables 2 and 3 respectively:

[0034] Table 2. Element composition of liquid vanadium-titanium slag from primary melting (%)

[0035] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 20.6 0.79 47.84 3.26 6.76 0.012 0.01 0.092 1.8

[0036] Table 3. Element composition of molten steel in the first molten phase (%)

[0037] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> Si Al S P C content / % 95.6 0.01 0.84 0.26 0.76 0.12 0.01 0.92

[0038] Step 4: High temperature granulation of liquid vanadium-titanium slag

[0039] Before the liquid vanadium-titanium-containing slag is transported to the high-temperature granulator, 8% by weight of petroleum coke and 15% by weight of titanium ore with a grade of 46 or above are added. After being mixed with the 1200°C high-temperature liquid vanadium-titanium-containing slag, it is transformed into high-temperature solid spherical particles through the high-temperature granulator. The temperature in the high-temperature granulator is 900°C, the diameter of the high-temperature solid spherical particles is 10-15mm, and the temperature of the spherical particles is 600°C. The high-temperature granulator here can recycle heat energy and transport it to step 2 for supplementary heat for coal-based reduction.

[0040] Step 5: Secondary melting reduction in electric furnace

[0041] The high-temperature granulated particles enter the insulation tank for insulation, and are lifted by the metallurgical crane into the electric furnace for secondary smelting reduction. The electric furnace smelts for 4 hours per furnace, and the smelting temperature is 1200℃. The vanadium-titanium magnetite is smelted to form high-titanium slag and liquid high-vanadium pig iron after secondary smelting. The high-titanium slag can be sold after cooling, and the liquid high-vanadium pig iron enters the next system. The composition of the high-titanium slag is shown in Table 4:

[0042] Table 4. Element composition of secondary smelting high titanium slag (%)

[0043] Element TFe V <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 2.69 0.086 64.56 4.399 9.12 0.01 0.01 0.124 2.42

[0044] Step 6: Converter Blowing

[0045] Liquid high-vanadium pig iron is blown in a converter to form semi-steel and vanadium slag. The blowing temperature is 1200℃ and the blowing time is 60min. The composition of semi-steel is shown in Table 5:

[0046] Table 5. Element analysis of secondary smelting semi-steel (%)

[0047] Element TFe V <![CDATA[TiO 2 ]]> Si Al S P C content / % 95.6 1.88 0.84 1.26 0.76 0.12 0.01 1.92

[0048] Vanadium slag V 2 O 5 Greater than 16%, iron recovery rate 95.89%.

[0049] Example 2

[0050] A vanadium-titanium magnetite smelting process specifically comprises the following steps:

[0051] Step 1: Grinding of vanadium-titanium magnetite

[0052] The vanadium-titanium magnetite ore is crushed and ground, and the grinding particle size is required to be below 200 mesh, accounting for 80%. Among them, the composition of vanadium-titanium magnetite is shown in Table 6:

[0053] Table 6. Element composition of vanadium-titanium magnetite ore (%)

[0054] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 48.03 0.37 22.31 1.52 3.15 0.011 0.015 0.043 0.84

[0055] Step 2: Coal-based reduction in rotary kiln

[0056] The crushed vanadium-titanium magnetite is added with 40% coal powder by weight and put into the rotary kiln. The mixed material is roasted in the rotary kiln for 2 hours at a roasting temperature of 900°C.

[0057] Step 3: Electric furnace primary melting

[0058] The roasted and reduced vanadium-titanium magnetite is transported to the electric furnace. The three electrodes of the electric furnace convert the electrical energy into heat energy to melt the vanadium-titanium magnetite. The electric furnace smelts for 4 hours per furnace at a smelting temperature of 1200°C. The vanadium-titanium magnetite is melted once to form molten steel and liquid vanadium-titanium slag. The molten steel is cooled to form steel products, and the liquid vanadium-titanium slag enters the next system. The components of the liquid vanadium-titanium slag and molten steel are shown in Tables 7 and 8 respectively:

[0059] Table 7. Element composition of liquid vanadium-titanium slag from primary melting (%)

[0060] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 19.2 0.83 48.32 3.35 6.85 0.014 0.01 0.096 1.84

[0061] Table 8. Element composition of molten steel in the first molten phase (%)

[0062] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> Si Al S P C content / % 96.3 0.01 0.64 0.21 0.64 0.10 0.01 0.72

[0063] Step 4: High temperature granulation of liquid vanadium-titanium slag

[0064] Before the liquid vanadium-titanium-containing slag is transported to the high-temperature granulator, 10% by weight of petroleum coke and 20% by weight of titanium ore with a grade of 46 or above are added. After being mixed with the 1000°C high-temperature liquid vanadium-titanium-containing slag, it is transformed into high-temperature solid spherical particles through the high-temperature granulator. The temperature in the high-temperature granulator is 800°C, the diameter of the high-temperature spherical particles is 10-15mm, and the temperature of the spherical particles is 500°C. The high-temperature granulator here can recycle heat energy and transport it to step 2 for heat supplement for coal-based reduction.

[0065] Step 5: Secondary melting reduction in electric furnace

[0066] The high-temperature granulated particles enter the insulation tank for lifting and insulation, and are then subjected to secondary melting reduction by the metallurgical crane electric furnace. The electric furnace smelts for 3 hours per furnace, and the smelting temperature is 1000°C. The vanadium-titanium magnetite is subjected to secondary melting to form high-titanium slag and liquid high-vanadium pig iron. The high-titanium slag can be sold after cooling, and the liquid high-vanadium pig iron enters the next system. The composition of the high-titanium slag is shown in Table 9:

[0067] Table 9. Element composition of secondary smelting high titanium slag (%)

[0068] Element TFe V <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 2.31 0.092 67.65 4.358 9.62 0.01 0.01 0.126 2.83

[0069] Step 6: Converter Blowing

[0070] Liquid high-vanadium pig iron is blown in a converter to form semi-steel and vanadium slag. The blowing temperature is 1250℃ and the blowing time is 50min. The composition of semi-steel is shown in Table 10:

[0071] Table 10. Element analysis of secondary smelting semi-steel (%)

[0072] Element TFe V <![CDATA[TiO 2 ]]> Si Al S P C content / % 95.3 1.92 0.92 1.28 0.78 0.14 0.01 1.96

[0073] Vanadium slag V 2 O 5 Greater than 16%, iron recovery rate 95.14%.

[0074] Example 3

[0075] A vanadium-titanium magnetite smelting process specifically comprises the following steps:

[0076] Step 1: Grinding of vanadium-titanium magnetite

[0077] The vanadium-titanium magnetite ore is crushed and ground, and the grinding particle size is required to be below 200 mesh, accounting for 80%. Among them, the composition of vanadium-titanium magnetite is shown in Table 11:

[0078] Table 11. Element composition of vanadium-titanium magnetite ore (%)

[0079] TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg 48.03 0.37 22.31 1.52 3.15 0.011 0.015 0.043 0.84

[0080] Step 2: Coal-based reduction in rotary kiln

[0081] The crushed vanadium-titanium magnetite is added with 38% coal powder by weight and put into the rotary kiln. The mixed material is roasted in the rotary kiln for 1.5 hours at a roasting temperature of 850°C.

[0082] Step 3: Electric furnace primary melting

[0083] The roasted and reduced vanadium-titanium magnetite is transported to the electric furnace. The three electrodes of the electric furnace convert the electrical energy into heat energy to melt the vanadium-titanium magnetite. The electric furnace smelts for 5 hours per furnace at a smelting temperature of 1300°C. The vanadium-titanium magnetite is melted once to form molten steel and liquid vanadium-titanium slag. The molten steel is cooled to form steel products, and the liquid vanadium-titanium slag enters the next system. The components of the liquid vanadium-titanium slag and molten steel are shown in Tables 12 and 13 respectively:

[0084] Table 12. Element composition of liquid vanadium-titanium slag from primary melting (%)

[0085] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 20.1 0.81 48.08 3.31 6.81 0.013 0.01 0.094 1.82

[0086] Table 13. Element composition of molten steel in the first melt (%)

[0087] Element TFe <![CDATA[V 2 THE 5 ]]> <![CDATA[TiO 2 ]]> Si Al S P C content / % 95.9 0.01 0.73 0.24 0.72 0.11 0.01 0.83

[0088] Step 4: High temperature granulation of liquid vanadium-titanium slag

[0089] Before the liquid vanadium-titanium-containing slag is transported to the high-temperature granulator, 9% by weight of petroleum coke and 18% by weight of titanium ore with a grade of 46 or above are added. After being mixed with the 1100°C high-temperature liquid vanadium-titanium-containing slag, it is transformed into high-temperature solid spherical particles through the high-temperature granulator. The temperature in the high-temperature granulator is 850°C, the diameter of the high-temperature spherical particles is 10-15mm, and the temperature of the spherical particles is 550°C. The high-temperature granulator here can recycle heat energy and transport it to step 2 for supplementary heat for coal-based reduction.

[0090] Step 5: Secondary melting reduction in electric furnace

[0091] The particles after high-temperature granulation are kept warm in an insulation tank and lifted by a metallurgical crane into an electric furnace for secondary smelting reduction. The electric furnace smelts for 3.5 hours per furnace at a smelting temperature of 1100°C. The vanadium-titanium magnetite is smelted to form high-titanium slag and liquid high-vanadium pig iron after secondary smelting. The high-titanium slag can be sold after cooling, and the liquid high-vanadium pig iron enters the next system. The composition of the high-titanium slag is shown in Table 14:

[0092] Table 14. Element composition of secondary smelting high titanium slag (%)

[0093] Element TFe V <![CDATA[TiO 2 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> S P Ca Mg content / % 2.45 0.089 66.12 4.373 9.44 0.01 0.01 0.125 2.62

[0094] Step 6: Converter Blowing

[0095] Liquid high-vanadium pig iron is blown in a converter to form semi-steel and vanadium slag. The blowing temperature is 1250℃ and the blowing time is 50min. The composition of semi-steel is shown in Table 15:

[0096] Table 15. Element analysis of secondary molten steel (%)

[0097] Element TFe V <![CDATA[TiO 2 ]]> Si Al S P C content / % 95.4 1.9 0.88 1.27 0.77 0.13 0.01 1.94

[0098] Vanadium slag V 2 O 5 Greater than 16%, iron recovery 95.36%.

Claims

1. A vanadium-titanium magnetite smelting process, characterized in that: The following steps are involved: Step 1: Grinding of vanadium-titanium magnetite The vanadium-titanium magnetite ore is crushed and ground; Step 2: Coal-based reduction in rotary kiln The crushed vanadium-titanium magnetite is added with coal powder and fed into a rotary kiln, where the mixture is roasted; Step 3: Electric furnace primary melting The roasted and reduced vanadium-titanium magnetite is transported to an electric furnace, and the electrodes of the electric furnace convert the electrical energy into heat energy to melt the vanadium-titanium magnetite once, forming molten steel and liquid vanadium-titanium slag. The molten steel is cooled to form steel products, and the liquid vanadium-titanium slag enters the next system; Step 4: High temperature granulation of liquid vanadium-titanium slag After the liquid vanadium-titanium-containing slag is transported to the high-temperature granulator, petroleum coke and titanium ore are added, and after being mixed with the high-temperature liquid vanadium-titanium-containing slag, it is transformed into high-temperature solid spherical particles through the high-temperature granulator; Step 5: Secondary melting reduction in electric furnace The high-temperature solid spherical particles enter the insulation tank for insulation, and then are transferred to the electric furnace for secondary smelting reduction to form high-titanium slag and liquid high-vanadium pig iron. The high-titanium slag can be sold after cooling, and the liquid high-vanadium pig iron enters the next system; Step 6: Converter Blowing Liquid high-vanadium pig iron is blown in a converter to form semi-steel and vanadium slag.

2. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step 1, the iron content of the vanadium-titanium magnetite ore is 30%-50%, and the vanadium content is 0.2%-1.5%; Grinding particle size below 200 mesh accounts for more than 80%.

3. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step 2, the amount of coal powder added is 30% to 40%; The mixed material is calcined at a temperature of 800°C-900°C and for a time of 1h-2h.

4. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step 3, the electric furnace smelting time is 4h-6h, and the smelting temperature is 1200℃-1400℃; The iron content in molten steel is greater than 95%.

5. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step 4, the amount of petroleum coke added is 8%-10%; the amount of titanium ore added is 15%-20% of titanium ore with a grade of 46 or above.

6. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step 4, the temperature of the high-temperature liquid vanadium-titanium slag is 1000° C.-1200° C.; The temperature of high-temperature solid spherical particles is 500℃-600℃, and the particle size is 10mm-15mm; The temperature of the high-temperature granulator is 800℃-900℃; the high-temperature granulator recovers heat energy and transmits it to the rotary kiln for heat supplement for coal-based reduction.

7. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step 5, the holding temperature is 500° C. to 600° C.; During the secondary melting reduction process, the electric furnace is used for 3-4 hours per furnace, and the melting temperature is 1000℃-1200℃; The vanadium content in liquid high-vanadium pig iron is 6%-8%.

8. The vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step six, the blowing temperature is 1200° C.-1250° C., and the blowing time is 50 min-60 min.

9. A vanadium-titanium magnetite smelting process according to claim 1, characterized in that: In step six, the iron content in the semi-steel is higher than 95%, and the V2O5 content in the vanadium slag is higher than 16%.