High-entropy alloy coating material resistant to oxidation at high temperature of 1200 DEG C and preparation and application of high-entropy alloy coating material

Through high-entropy alloy coating materials of Fe, Y, Hf and other elements, combined with supersonic plasma spraying technology, the problems of coating stability and high cost at high temperatures of 1200°C are solved, and efficient oxidation resistance and simplified preparation processes are achieved. .

CN118726894APending Publication Date: 2024-10-01ANSTEEL BEIJING RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410776044.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technology is difficult to provide stable thermal barrier coating materials at high temperatures of 1200°C, leading to premature failure of the coating, high costs, and complex preparation processes.

Method used

Using high-entropy alloy coating materials of Fe: 23% ~ 26%, Y: 0.015 ~ 0.025%, Hf: 0.015 ~ 0.025%, CoNiCrAlFe-YHf high-entropy alloy powder is prepared through vacuum arc melting and vacuum argon atomization, and Deposited on a heat-resistant alloy substrate using supersonic plasma spraying technology.

Benefits of technology

It achieves a high-entropy alloy coating with a smooth surface without peeling, a uniform and dense oxide layer and a single high-entropy alloy coating at a high temperature of 1200°C, which reduces the alloy cost, simplifies the preparation process, and significantly improves the oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726894A_ABST
    Figure CN118726894A_ABST
Patent Text Reader

Abstract

The invention relates to a high-entropy alloy coating material capable of resisting high-temperature oxidation at 1200 DEG C. The high-entropy alloy coating material comprises the following elements in percentage by atom: 23%-26% of Fe, 0.015%-0.025% of Y, 0.015%-0.025% of Hf and the balance of Co, Ni, Cr and Al with equal atomic ratio. The preparation process comprises the following steps: 1) smelting and die casting according to element components to obtain a high-entropy alloy cast ingot; (2) the high-entropy alloy cast ingot is prepared into CoNiCrAlFe-YHf high-entropy alloy powder through vacuum argon atomization; and (3) high-entropy alloy powder is deposited on the pretreated heat-resisting alloy matrix through supersonic plasma spraying, and the coating is prepared. The high-entropy alloy coating can keep extremely high phase stability at the high temperature of 1200 DEG C or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a coating material, in particular to a high entropy alloy coating material resistant to 1200°C high-temperature oxidation. Background Art

[0002] With the continuous development of aviation turbine engines and gas turbines towards high thrust-to-weight ratio and high flow ratio, the inlet temperature of the turbine is required to continue to increase. Coating thermal barrier coating on the surface of high-temperature alloy of blades is an inevitable choice. The thermal barrier coating relies on the outermost ceramic layer to isolate most of the heat, and uses the middle bonding layer to bond the blade substrate and the ceramic layer. The bonding layer can reduce the interfacial stress and prevent the ceramic layer from peeling off prematurely during use. A thin and dense layer of Al2O3 will form on the surface of the bonding layer at high temperature to inhibit its further oxidation. As Al2O3 further thickens, the continuous accumulation of thermal stress will cause it to wrinkle and crack, leading to the failure of the coating.

[0003] The current bonding layer materials are mainly MCrAlY (M is Co and Ni) and NiPtAl coatings. Among them, the Al content in the MCrAlY coating is generally controlled at 8-12wt.%, and the service temperature is below 1100℃; when serving above 1100℃, the coating will oxidize rapidly and form non-protective spinel oxides, resulting in premature failure of the coating. NiPtAl coating slows down the oxidation rate by increasing the Al content (50%-80%). The coating can work at 1150-1200℃, but a large amount of Al will form severe interdiffusion with the high-temperature alloy blades at high temperatures, greatly reducing the creep performance of the blades.

[0004] As the operating temperature of turbines continues to increase, there is an urgent need for thermal barrier coating bonding layer materials that can stably work at 1200°C. The inherent lattice distortion effect and hysteresis diffusion effect of high entropy alloys help to slow down the outward diffusion of Al, reduce its oxidation rate at high temperatures, and extend the service life of the coating. Therefore, it is very promising to develop a bonding layer material that can serve for a long time at 1200°C based on the special effects of high entropy alloys.

[0005] The invention patent with the publication number CN114411081A discloses a Y / Hf doped AlCoCrFeNiSi high entropy thermal barrier bonding layer and its preparation method. The invention patent selects Y and Hf elements with a mass ratio of 0.02at.%, and high-purity Al, Co, Cr, Fe, Ni, and Si with equal atomic ratios. First, the raw materials are melted into ingots by vacuum arc melting, and then the ingots are atomized into powders by vacuum argon gas, and finally sprayed. The deposition rate of the coating is high and the adhesion is good. The thermal expansion coefficient is much smaller than that of the MCrAlY coating at high temperature, and the stress change is more gentle. However, the invention only shows that this coating does not undergo phase change after long-term heat treatment at 1200℃, and points out that it has better oxidation resistance and corrosion resistance than traditional MCrAlY coating at the same temperature. The oxidation rate of long-term isothermal oxidation and cyclic oxidation at 1200℃ is not given, and its oxidation resistance at 1200℃ is not actually tested. It only shows that its thermal expansion coefficient is low.

[0006] The invention patent with the publication number CN113881884A discloses a long-life anti-oxidation high-entropy bonding layer material and its preparation method. The composition of the material is Al, Co, Cr, Fe, Ni in equal atomic ratios, and 0.5wt.% of active elements Y and Hf are added. The preparation method is: prepare the alloy block by vacuum magnetic levitation melting technology, grind it into powder by crusher and planetary ball mill; sieve the powder by standard sieve; treat the surface of nickel-based high-temperature alloy matrix; prepare the transition layer on the surface of nickel-based high-temperature alloy by atmospheric plasma spraying; prepare Y / Hf modified AlCoCrFeNi high-entropy bonding layer on the surface of transition layer by atmospheric plasma spraying. The bonding layer material has excellent high-temperature structural stability, and its surface is intact and has no peeling after 200 cycles of oxidation at 1150℃ and 100 cycles at 1200℃. However, the bonding layer needs to be coated on a transition layer of NiCoCrAlY (composition is 47.5wt% Ni, 23wt% Co, 16.7wt% Cr, 12.3wt% Al, 0.5wt% Y). On the one hand, the technical requirements are very high, and on the other hand, the cost of thermal barrier coating is greatly increased.

[0007] The invention patent with publication number CN116145012A discloses a high entropy alloy with high temperature oxidation resistance and its preparation method. The composition of the bonding layer material is: Al 16-22at.%, Co 15-20at.%, Cr 15-20at.%, Fe15-20at.%, Ta 0.4-1at.%, Y / Hf 0-0.12at.%, and the balance Ni. The preparation method is: weigh the raw materials according to the molar percentage of the elements; place the raw materials in a crucible and put them into a vacuum arc melting furnace for melting. The bonding layer can serve for more than 670 hours in an air atmosphere at 1100°C. It not only has a low oxidation rate and high anti-stripping performance, but also does not generate other oxides such as spinel. However, the bonding layer has a high content of Ta element, which is a precious metal, making the cost of the material high. In addition, the alloy has good long-term oxidation resistance only at 1100°C, and the service temperature is lower than 1200°C.

[0008] The invention patent with the authorization number CN114703440B discloses a nano-oxide dispersion-strengthened high-entropy alloy bonding layer and its preparation method, which includes an AlCoCrFeNi~YHf high-entropy alloy bonding layer with an equiatomic ratio attached to the surface of a high-temperature alloy substrate and in-situ dispersed nano-oxides, accounting for 10-20% of the total volume. The preparation method is: ball milling the AlCoCrFeNi~YHf high-entropy alloy to obtain AlCoCrFeNi~YHf high-entropy alloy powder; using active combustion high-velocity gas spraying technology to spray the powder on the surface of the high-temperature alloy substrate to obtain a nano-oxide dispersion-strengthened high-entropy alloy bonding layer. In this invention, the nano-oxide has a low thermal expansion coefficient, which can reduce the thermal expansion mismatch between the bonding layer and the oxide film, reduce residual stress, and improve the anti-stripping ability of the oxide film. After the coating was cyclically oxidized at 1100℃ for 1000h, the oxide film did not show any form of spalling. However, the preparation of the bonding layer is technically difficult. First, there are strict restrictions on the process parameters of active combustion high-velocity fuel gas spraying; second, there are strict restrictions on the size and volume fraction of the formed nano-oxides, which seriously limits the success rate of the preparation of the bonding layer.

[0009] The invention patent with the authorization number CN111663070B discloses a high-temperature oxidation-resistant AlCoCrFeNiSiY high-entropy alloy and its preparation method. Compared with the traditional NiCoCrAlY, the high-entropy alloy has increased the alloying elements Fe and Si, and made significant adjustments in content: Al 18%, Co 15%, Cr 15%, Fe 16.8%, Ni 32.9%, Si 2%, Y0.3% (atomic percentage). The preparation method is: vacuum melting the raw materials and homogenizing them in an environment of 1200±30℃ for 6 hours. The high-entropy alloy shows better resistance to high-temperature oxidation weight gain under 1150℃ cyclic oxidation conditions. Its oxide film is uniform and dense, and the bonding state is good. However, the alloy is not sprayed on the surface of the high-temperature alloy, and its bonding with the high-temperature alloy is unknown. And its good oxidation resistance is only at 1150℃, not 1200℃.

[0010] The invention patent with the authorization number CN111809094B discloses a high-entropy alloy resistant to high-temperature oxidation, a thermal barrier coating and a preparation method thereof. The high-entropy alloy is prepared by adding alloying elements Fe, Ta and Hf to NiCoCrAlY to obtain AlCoCrFeNiTaHfY high-entropy alloy (Al 16-22%, Co 14-20%, Cr 14-20%, Fe 5-8%, Ni 38-45%, Ta 1-2%, Hf 0.02-0.1%, Y 0.2-0.5%), and its configuration entropy is higher than 1.5R. The preparation method is: firstly, the material is placed in a vacuum arc furnace for smelting, then the ingot is prepared into powder, the high-temperature alloy is surface pretreated, and the high-entropy alloy powder is deposited on the high-temperature alloy substrate by supersonic plasma spraying. The high-entropy alloy bonding layer shows a lower thermally generated oxide growth rate under 1150°C cyclic oxidation conditions, and its oxide layer is uniform and dense, and has a good bonding state with the alloy substrate. However, the high-entropy alloy has high Ni and Ta contents, which results in high alloy cost and a long-term service temperature of 1150°C. Summary of the invention

[0011] The technical problem to be solved by the present invention is to provide a high entropy alloy coating material resistant to high-temperature oxidation at 1200°C, the material has low cost, simple preparation process, and good organizational stability when in service at 1200°C.

[0012] To achieve the above object, the present invention adopts the following technical solutions:

[0013] A high entropy alloy coating material resistant to high temperature oxidation at 1200 DEG C, wherein the atomic percentage of elements is: Fe: 23%-26%, Y: 0.015-0.025%, Hf: 0.015-0.025%, and the rest is Co, Ni, Cr, Al in equal atomic ratio.

[0014] A process for preparing a high entropy alloy coating resistant to high temperature oxidation at 1200°C, the specific steps comprising:

[0015] 1) Melting and casting according to the elemental composition to obtain a high entropy alloy ingot;

[0016] 2) preparing the high entropy alloy ingot into CoNiCrAlFe-YHf high entropy alloy powder by vacuum argon atomization;

[0017] 3) Using supersonic plasma spraying, high entropy alloy powder is deposited on the pretreated heat-resistant alloy substrate to prepare a coating.

[0018] The step 1) is performed by smelting in a vacuum arc furnace.

[0019] In the step 1), during the casting process, the casting mold is turned over 4 to 5 times to make the composition of the ingot uniform.

[0020] The step 3) pretreatment process of the heat-resistant alloy substrate: grinding the surface of the heat-resistant alloy substrate to ensure a smooth and flat surface.

[0021] High entropy alloy coating material resistant to high temperature oxidation at 1200°C is used as a bonding layer for thermal barrier coatings.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The high entropy alloy coating material of the present invention is doped with trace amounts of Y and Hf elements, which can effectively delay the diffusion of elements and significantly improve the high-temperature oxidation resistance of the alloy. A large amount of Fe (Fe content of 23-26 at.%) is added to the high entropy alloy coating material, the unit price of Fe element is low, and the unit prices of Y and Hf elements are high, which greatly reduces the cost of the high entropy alloy coating material.

[0024] 2. The high entropy alloy coating material of the present invention is composed of a pure BCC phase, which contains an ordered B2 phase rich in Ni and Al and a disordered A2 phase rich in Cr and Fe. The A2 phase and the B2 phase are stacked in a lamellar structure, which not only has high thermal stability, but also has a very slow element diffusion rate, so that the high entropy alloy coating can maintain extremely high phase stability at high temperatures above 1200°C.

[0025] 3. The high entropy alloy coating material of the present invention has excellent oxidation resistance in an air environment of 1200°C, and the oxidation rate of the high entropy alloy coating is very slow (the growth rate of the oxidation layer is about 2.77×10 -13 cm 2 s -1). It is deposited on the heat-resistant alloy substrate to form a coating. The surface is flat and has no peeling after isothermal oxidation at 1200℃ for 500h and cyclic oxidation at 1200℃ for 100h. The oxide layer (Al2O3) formed on the surface is uniform, dense and single. The Al content in the alloy is reduced in the material, which reduces the mutual diffusion between the high entropy alloy coating and the heat-resistant alloy substrate at high temperatures above 1200℃, thereby extending the service life. At the same time, the alloy coating material has good adhesion to the heat-resistant alloy substrate, and the deposition rate is high and flat.

[0026] 4. High entropy alloy coating materials are used in coatings or thermal barrier coating bonding layers of turbine and gas turbine blades, making it possible for turbines and gas turbines to serve at 1200°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the metallographic structure diagram of high entropy alloy coating material.

[0028] Figure 2 This is the actual morphology of the high entropy alloy coating after isothermal oxidation at 1200℃.

[0029] Figure 3 This is the actual morphology of the high entropy alloy coating after cyclic oxidation at 1200℃.

[0030] Figure 4 This is the XRD spectrum of the high entropy alloy coating after isothermal oxidation at 1200℃ in air environment for 500h.

[0031] Figure 5 It is the oxidation rate curve diagram of the embodiment and the comparative example. DETAILED DESCRIPTION

[0032] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0033] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means more than two.

[0034] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0035] A high entropy alloy coating material resistant to high temperature oxidation at 1200 DEG C, wherein the atomic percentage of elements is: Fe: 23%-26%, Y: 0.015-0.025%, Hf: 0.015-0.025%, and the rest is Co, Ni, Cr, Al in equal atomic ratio.

[0036] A process for preparing a high entropy alloy coating resistant to high temperature oxidation at 1200°C, the specific steps comprising:

[0037] 1) Melting and casting according to the elemental composition to obtain a high entropy alloy ingot;

[0038] 2) preparing the high entropy alloy ingot into CoNiCrAlFe-YHf high entropy alloy powder by vacuum argon atomization;

[0039] 3) Using supersonic plasma spraying, high entropy alloy powder is deposited on the pretreated heat-resistant alloy substrate to prepare a coating.

[0040] The step 1) is performed by smelting in a vacuum arc furnace.

[0041] In the step 1), during the casting process, the casting mold is turned over 4 to 5 times to make the composition of the ingot uniform.

[0042] The step 3) of pre-treating the heat-resistant alloy substrate includes grinding, sandblasting, ultrasonication and drying.

[0043] High entropy alloy coating material resistant to high temperature oxidation at 1200°C is used as a bonding layer for thermal barrier coatings.

[0044] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

[0045] In order to make the purpose, technical scheme and technical effect of the present invention clearer, the technical scheme in the embodiment of the present invention is now clearly and completely described. However, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. In combination with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Example

[0047] The high entropy alloy coating resistant to high temperature oxidation at 1200° C. has an atomic percentage (at.%) of Fe: 24%, Y: 0.02%, Hf: 0.02%, and the rest are Co, Ni, Cr, and Al in equal atomic ratios.

[0048] A method for preparing a high entropy alloy coating, comprising:

[0049] 1) Use vacuum arc furnace to melt and mold according to element composition. The vacuum degree of vacuum arc furnace is 5×10 -3 Pa, the working current is 200-220A, the working power is 45kW, the furnace cooling time is 50min, and a high entropy alloy ingot is obtained; during the mold casting process, the mold is turned over 4-5 times to make the ingot composition uniform.

[0050] 2) The high entropy alloy ingot is prepared into CoNiCrAlFe-YHf high entropy alloy powder by vacuum argon atomization; the powder is required to be nearly spherical with good fluidity.

[0051] 3) The surface of the heat-resistant alloy substrate IN718 was polished to 2000# with sandpaper, and then the surface was roughened by sandblasting with a sandblasting machine. The nickel-based alloy was then ultrasonicated in alcohol and dried for later use.

[0052] 4) Use supersonic plasma spraying to deposit the high entropy alloy powder on the pretreated heat-resistant alloy substrate, the deposition parameters are: voltage 150-200V, current 350-450A, argon flow rate 90L / min, hydrogen flow rate 20L / min, spraying distance 100-120mm, spray gun moving speed 500-600mm / s, to prepare a coating with a coating thickness of 100-200μm.

[0053] The oxidation resistance of nickel-based alloy specimens after depositing high entropy alloy coating was evaluated in an air environment at 1200℃.

[0054] 1) Isothermal oxidation at 1200℃: First, heat the muffle furnace to 1200℃, then put the sample in, and start timing after the temperature rises to 1200℃ again. Take out the sample after 1h, 9h, 25h, 100h, and 500h, respectively. After cooling in the air, observe the surface morphology of the sample. The results of isothermal oxidation at 1200℃ show that after isothermal oxidation at 1200℃ for 500h, the surface of the high entropy alloy coating is smooth without peeling, and the surface oxide layer is uniform and dense, such as Figure 2 shown.

[0055] 2) 1200℃ cyclic oxidation: Place the sample in a muffle furnace at 1200℃, and start timing after the temperature is raised to 1200℃ again. Take it out after 1 hour, cool it in air for 10 minutes, and then put it back in the muffle furnace at 1200℃. Repeat this process 100 times. The results of 1200℃ cyclic oxidation show that after 100h of 1200℃ cyclic oxidation, the surface of the high entropy alloy coating is smooth and has no peeling. The surface oxide layer is uniform and dense, such as Figure 3 shown.

[0056] The sample after isothermal oxidation at 1200℃ for 500h was placed in an XRD instrument for testing. The test results are as follows: Figure 4 As shown in the figure, the XRD results show that after the high entropy alloy coating is isothermally oxidized at 1200℃ for 500h, only Al2O3 single oxide is formed on the surface, and no oxides of other components are generated.

[0057] The above example results show that the service temperature of the high entropy alloy coating prepared by the present invention can reach 1200°C. After oxidation at 1200°C, the surface oxide layer is uniform, dense and single, while the service temperature of the traditional MCrAlY coating is only 1100°C.

[0058] The sample after isothermal oxidation at 1200℃ for 500h was ground to 2000# with sandpaper and polished. The oxide layer on the high entropy alloy coating was observed and its thickness was measured by SEM, and the oxidation rate of the high entropy alloy coating was calculated. The calculation formula is: Δh 2 =2k ht, where Δh is the thickness of the oxide layer, t is the oxidation time, k h is the oxidation rate. The results are as follows Figure 4 As shown in FIG. 1 , the oxidation rate of the high entropy alloy coating of the present invention in an air environment at 1200°C is about 2.77×10 -13 cm 2 s -1 .

[0059] Comparative Example

[0060] A CoNiCrAlFe high entropy alloy coating material with equal atomic ratio, wherein the atomic percentage (at.%) of the elements is: Y: 0.02%, Hf: 0.02%, and the rest is Co, Ni, Cr, Al, and Fe with equal atomic ratio. The CoNiCrAlFe high entropy alloy coating with equal atomic ratio is prepared by the method of the embodiment.

[0061] The same isothermal oxidation experiment was carried out at 1200℃ to test its oxidation rate. The oxidation rate curve is shown in Figure 5 As shown in the figure, the oxidation rate of the CoNiCrAlFe high entropy alloy coating with the same atomic ratio in the comparative example in an air environment at 1200℃ is about 3.98×10 -13 cm 2 s -1 .

[0062] The oxidation rate of the CoNiCrAlFe high entropy alloy coating with an equiatomic ratio at 1200°C is approximately 1.44 times that of the high entropy alloy coating with a high Fe content of the present invention, which proves that the high entropy alloy coating with a high Fe content of the present invention has more excellent antioxidant properties.

[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high entropy alloy coating material resistant to high temperature oxidation at 1200°C, characterized in that: The atomic percentage of the elements is: Fe: 23% to 26%, Y: 0.015 to 0.025%, Hf: 0.015 to 0.025%, and the rest are Co, Ni, Cr, and Al in equal atomic ratios.

2. The process for preparing a high entropy alloy coating resistant to high temperature oxidation at 1200°C according to claim 1, characterized in that: The specific steps include: 1) Melting and casting according to the elemental composition to obtain a high entropy alloy ingot; 2) preparing the high entropy alloy ingot into CoNiCrAlFe-YHf high entropy alloy powder by vacuum argon atomization; 3) Using supersonic plasma spraying, high entropy alloy powder is deposited on the pretreated heat-resistant alloy substrate to prepare a coating.

3. The process for preparing a high entropy alloy coating resistant to high temperature oxidation at 1200°C according to claim 2, characterized in that: The step 1) is performed by smelting in a vacuum arc furnace.

4. The process for preparing a high entropy alloy coating resistant to high temperature oxidation at 1200°C according to claim 2, characterized in that: In the step 1), during the casting process, the casting mold is turned over 4 to 5 times to make the composition of the ingot uniform.

5. The process for preparing a high entropy alloy coating resistant to high temperature oxidation at 1200°C according to claim 2, characterized in that: The step 3) pretreatment process of the heat-resistant alloy substrate: grinding the surface of the heat-resistant alloy substrate to ensure a smooth and flat surface.

6. The high entropy alloy coating material resistant to high temperature oxidation at 1200°C according to claim 1, characterized in that: High entropy alloy coating materials are used as bonding layers of thermal barrier coatings.

Citation Information

Cited By

  • High-temperature oxidation-resistant high-entropy alloy capable of remarkably reducing sigma high-temperature brittle phase precipitation and preparation method of high-temperature oxidation-resistant high-entropy alloy

    CN118621198A