High-temperature anti-oxidation coating suitable for TiAl alloy and preparation method of high-temperature anti-oxidation coating

The Ti-Al-Cr-Nb-Si-Y coating is prepared on the surface of TiAl alloy through multi-arc ion plating technology, which solves the problems of poor bonding force and easy peeling in the preparation of existing high-temperature anti-oxidation coating of TiAl alloy, and achieves high-temperature The improvement of antioxidant properties and reduction of production costs make it suitable for batch processing.

CN118726918AActive Publication Date: 2024-10-01NORTHWESTERN POLYTECHNICAL UNIV +1

Patent Information

Application Number
CN202411037520.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-01
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing TiAl alloy high-temperature anti-oxidation coating preparation process has problems such as poor bonding force, easy peeling, and impact on the matrix structure. Moreover, the commonly used alloying method has a long research cycle and high cost, which affects the comprehensive mechanical properties of the alloy.

Method used

Multi-arc ion plating technology is used to prepare the Ti-Al-Cr-Nb-Si-Y coating on the TiAl alloy surface. The nanometer microstructure is formed through pretreatment and the TiaAlbCrcNbdSieYf multi-element alloy target is used to ensure the uniform density and high bonding of the coating. force.

Benefits of technology

The high-temperature anti-oxidation coating on the surface of the TiAl alloy has good adhesion and high-temperature anti-oxidation properties, which reduces production costs and is suitable for batch processing. There is no peeling or peeling after constant temperature oxidation at 850°C for 600 hours, which significantly improves the performance of the TiAl alloy. high temperature service temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726918A_ABST
    Figure CN118726918A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature anti-oxidation coating suitable for a TiAl alloy and a preparation method of the high-temperature anti-oxidation coating. The method comprises the steps that firstly, a prefabricated TiAl alloy base material is obtained through treatment; secondly, a Ti Al Cr < c > Nb < d > Si < e > Y < f > multi-element alloy target material is prepared; thirdly, plasma etching is carried out on the prefabricated TiAl alloy base material; and fourthly, the TiAl alloy with the Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating deposited on the surface is obtained through multi-arc ion plating. According to the method, the Ti-Al-Cr-Nb-Si-Y coating is prepared on the surface of the TiAl alloy through the multi-arc ion plating technology, the coating is uniform and compact in structure, good in combination with the matrix TiAl alloy, high in hardness and good in high-temperature oxidation resistance, and the preparation technology is simple, high in operability, low in production cost and beneficial to large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature anti-oxidation coating preparation, and in particular relates to a high-temperature anti-oxidation coating suitable for TiAl alloy and a preparation method thereof. Background Art

[0002] Titanium aluminum alloy has the advantages of low density, large elastic modulus, high specific strength, high corrosion resistance, good high temperature oxidation resistance, good creep resistance, etc. It is widely used in the field of aerospace materials. However, when serving at high temperatures above 800°C, the limited oxidation resistance becomes an obstacle to the further application of titanium aluminum alloy. At present, the commonly used solution is to improve the high temperature oxidation resistance of the alloy by alloying and preparing surface coatings. However, the research cycle of the alloying method is long, the workload is large, the research cost is high, and the risk is high. The overall alloying will also seriously affect the comprehensive mechanical properties of the alloy, especially increase brittleness and reduce fatigue performance. Therefore, it is necessary to prepare a coating on the surface of titanium aluminum alloy to improve its high temperature oxidation resistance.

[0003] At present, the preparation methods for high-temperature anti-oxidation coatings on the surface of TiAl alloys mainly include diffusion infiltration, laser cladding, double glow plasma infiltration, atmospheric plasma spraying, physical vapor deposition, etc. The deposition rate of diffusion infiltration coating is low, the preparation time is long, and the reaction temperature is high, which may affect the matrix structure; laser cladding has a large temperature difference near the molten pool area, resulting in poor coating adhesion, easy cracking and peeling; double glow plasma infiltration equipment has high requirements, which is not conducive to the processing of parts with complex sizes; atmospheric plasma spraying is formed by powder materials in a molten or semi-molten state hitting the workpiece at high speed, and there are some inevitable pores and cracks between the powder particles. Physical vapor deposition can deposit coating materials on the surface of the substrate through evaporation, sputtering and other processes. This method can obtain high-density, low-porosity coatings, and the coating thickness is controllable. Among them, multi-arc ion plating technology is to ionize the gas or evaporated material through gas discharge under vacuum, and when the gas ions or evaporated material ions bombard at high speed, the evaporated material or its reactants are deposited on the parts to be plated. Since multi-arc ion plating technology can ensure the simultaneous existence of sputtering cleaning and deposition coating, it can effectively reduce the internal stress of the film, the film layer is dense, the film layer has strong adhesion, good winding performance, and high deposition rate. At the same time, the multi-arc ion plating equipment is simple, the process is highly repeatable, and the composition and thickness of the coating can be precisely controlled. Therefore, the use of multi-arc ion plating technology to prepare coatings on TiAl alloys is expected to become an effective method to improve their high-temperature oxidation resistance, which will further achieve the high-temperature service temperature of TiAl alloys. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a high-temperature anti-oxidation coating suitable for TiAl alloy in view of the shortcomings of the above-mentioned prior art. The method adopts a multi-arc ion plating process to prepare a Ti-Al-Cr-Nb-Si-Y coating on the surface of the TiAl alloy. The coating has a uniform and dense structure, is well bonded to the matrix TiAl alloy, has high hardness, and has good high-temperature anti-oxidation performance, thus solving the shortcomings of the existing preparation process of the high-temperature anti-oxidation coating on the surface of the TiAl alloy, such as poor bonding strength, easy peeling, and influence on the matrix structure.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a high-temperature anti-oxidation coating suitable for TiAl alloy, characterized in that the method comprises the following steps:

[0006] Step 1: Prefabrication of TiAl alloy substrate: After finishing the surface of the TiAl alloy, polishing treatment is performed, and then cleaning is performed until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying is performed to obtain a prefabricated TiAl alloy substrate;

[0007] Step 2: Preparation of multi-element alloy target: Prepare Ti a Al b Cr c Nb d Si e Y f The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment, wherein a, b, c, d, e, and f represent the atomic proportions of the corresponding elements, and a+b+c+d+e+f=1, 0.1≤a≤0.3, 0.5≤b≤0.6, 0.1≤c≤0.16, 0.03≤d≤0.04, 0.05≤e≤0.10, and f≈0.01;

[0008] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. a Al b Cr c Nb d Si e Y f The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 - 3 Pa, turn on the high-frequency plasma power supply, then introduce H2 to adjust the pressure in the vacuum chamber to 0.5Pa~2Pa, then apply bias to the prefabricated TiAl alloy substrate, and the formed electric field performs plasma etching on the TiAl alloy substrate to remove oxide impurities on the surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 0.5Pa~2Pa, and continue to perform plasma etching on the TiAl alloy substrate;

[0009] Step 4: multi-element coating deposition: an external electric field is applied to the TiAl alloy substrate after Ar gas plasma etching in step 3, and argon gas is introduced into the vacuum chamber to adjust the vacuum degree, and then the cathode target arc is started for multi-arc ion plating to obtain a TiAl alloy with a Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating deposited on the surface.

[0010] The above-mentioned method for preparing a high-temperature anti-oxidation coating suitable for TiAl alloy is characterized in that the finishing in step 1 is to use a machining center to perform precision milling on the surface of the TiAl alloy. The finishing operation reduces the difficulty of subsequent polishing and is suitable for batch substrate processing.

[0011] The above-mentioned method for preparing a high-temperature anti-oxidation coating suitable for TiAl alloy is characterized in that the cleaning process described in step one is: first use an industrial degreasing cleaning agent for degreasing cleaning, and then use deionized water and ethanol solution in turn for ultrasonic cleaning at 25°C to 40°C for 15min to 20min respectively.

[0012] The above-mentioned method for preparing a high-temperature anti-oxidation coating suitable for TiAl alloy is characterized in that in step three, the high-frequency plasma power supply is turned on to control the plasma voltage to 200V~500V, the vacuum chamber temperature is 200℃~400℃, the substrate bias voltage is set to 40V~60V when H2 is introduced for plasma etching, and the etching time is 10min, and the substrate bias voltage is set to 200V~600V when Ar gas is introduced for plasma etching, and the etching time is 30min~60min.

[0013] The plasma power source is the source of plasma. By applying a bias voltage, the directional impact of the plasma on the TiAl alloy substrate is increased. Under the combined action of the two, the TiAl alloy substrate is plasma-etched, which is conducive to the formation of a micro-nano structure on the substrate surface that is conducive to the bonding of the coating. Specifically, H2 is first introduced and a relatively low bias voltage is used. With the help of the reduction effect of H2, plasma etching is performed at a relatively high temperature to remove oxides and other impurities on the surface of the TiAl alloy substrate. Then, Ar gas is introduced and the bias voltage applied to the substrate surface is increased. The TiAl alloy substrate is plasma-etched to a greater depth, forming a nanostructure that is conducive to the bonding of the coating, thereby improving the bonding strength between the high-temperature anti-oxidation coating and the TiAl alloy substrate.

[0014] The above-mentioned method for preparing a high-temperature anti-oxidation coating suitable for TiAl alloy is characterized in that the voltage of the external electric field applied in step four is -100V to -350V, the vacuum degree is adjusted to 0.5Pa to 2Pa, the cathode arc current generated by the cathode target arc is 50A to 120A, the temperature of the multi-arc ion plating is maintained at 150°C to 400°C, and the time is 20min to 80min.

[0015] At the same time, the present invention also discloses a high-temperature anti-oxidation coating suitable for TiAl alloy, which is characterized in that it is prepared by the above method.

[0016] Compared with the prior art, the present invention has the following advantages:

[0017] 1. The present invention adopts multi-arc ion plating process to prepare high temperature oxidation resistant coating on the surface of TiAl alloy. a Al b Cr c Nb d Si e Y f Using the multi-element alloy as the target material, a Ti-Al-Cr-Nb-Si-Y coating was successfully deposited on the surface of the TiAl alloy substrate. The coating has a uniform and dense structure, is well bonded to the substrate, and has a hardness of up to 900 HV, which is 80% higher than that of the substrate.

[0018] 2. The present invention adopts Ti a Al b Cr c Nb d Si e Y f A multi-element alloy is used as a target to deposit a Ti-Al-Cr-Nb-Si-Y coating on the surface of a TiAl alloy substrate, wherein the corresponding proportions of Al, Cr, Si and Nb ensure that a dense and continuous Al2O3 film is formed on the surface of the coating, while also inhibiting the competitive oxidation of Ti. The introduction of the Si element improves the toughness of the coating, while the addition of the trace element Y increases the viscosity of the coating and improves the bonding strength between the coating and the substrate, thereby ensuring that the Ti-Al-Cr-Nb-Si-Y coating has good high-temperature oxidation resistance; ultimately, the Ti-Al-Cr-Nb-Si-Y coating prepared by the present invention has a unit area weight growth rate reduced by more than 60% compared with a substrate without a coating after constant temperature oxidation at 850°C for 600 hours, and there is no peeling or shedding phenomenon (the substrate without a coating has obvious peeling and flaking starting from oxidation for 5 hours), showing good high-temperature oxidation resistance.

[0019] 3. The present invention uses plasma etching to pre-treat the TiAl alloy substrate before depositing the Ti-Al-Cr-Nb-Si-Y coating to form a nano-microstructure on the substrate surface. The microstructure improves the bonding force between the surface coating and the substrate through a gripping effect.

[0020] 4. When prefabricating the TiAl alloy substrate, the present invention uses a machining center to perform precision milling on the TiAl alloy sample and then polishing it, which reduces the difficulty and working hours of subsequent manual polishing, is suitable for batch processing of the substrate, and significantly reduces the polishing time compared to conventional manual polishing.

[0021] 5. The preparation process of the present invention is simple, operable, and has low production cost, which is conducive to large-scale industrial application.

[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the EDS energy spectrum of the Ti-Al-Cr-Nb-Si-Y high temperature anti-oxidation coating prepared in Example 1 of the present invention.

[0024] Figure 2 This is a surface SEM morphology of the Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating prepared in Example 1 of the present invention.

[0025] Figure 3 The 600h constant temperature oxidation weight change curve of the TiAl alloy with Ti-Al-Cr-Nb-Si-Y high temperature anti-oxidation coating prepared in Examples 5 to 6 of the present invention and the TiAl alloy without coating.

[0026] Figure 4 This is a macroscopic photograph of the TiAl alloy with a substrate and a Ti—Al—Cr—Nb—Si—Y high-temperature anti-oxidation coating deposited on the surface used in Example 6 of the present invention after high-temperature oxidation for 600 hours. DETAILED DESCRIPTION

[0027] Example 1

[0028] This embodiment includes the following steps:

[0029] Step 1, prefabrication of TiAl alloy substrate: using a machining center to perform precision milling and finishing on the surface of the TiAl alloy, and then polishing, and then cleaning until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying to obtain a prefabricated TiAl alloy substrate; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil and clean, and then use deionized water and ethanol solution in turn at 25°C to 40°C for 15 minutes respectively;

[0030] Step 2: Preparation of multi-element alloy target: Prepare Ti 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0.1 Y 0.01The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment;

[0031] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0.1 Y 0.01 The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 -3 Pa, turn on the high-frequency plasma power supply, control the plasma voltage to 200V, then introduce H2 to adjust the pressure in the vacuum chamber to 1Pa, control the temperature of the vacuum chamber to 200°C, then apply a 40V base bias to the prefabricated TiAl alloy substrate, and use the formed electric field to perform plasma etching on the TiAl alloy substrate for 10min to remove oxide impurities on its surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 1Pa, and use a 500V base bias to perform plasma etching on the TiAl alloy substrate for 40min;

[0032] Step 4, multi-element coating deposition: apply an external electric field to -350V to the TiAl alloy after Ar gas plasma etching in step 3, introduce argon gas into the vacuum chamber to adjust the vacuum degree to 0.5Pa, and then start the cathode target arc for multi-arc ion plating. The cathode arc current is 50A, and the temperature of multi-arc ion plating is maintained at 150°C for 50min to obtain a TiAl alloy with a surface deposited Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating.

[0033] Figure 1 This is the EDS spectrum of the Ti-Al-Cr-Nb-Si-Y high temperature oxidation resistant coating prepared in this example. Figure 1 It can be seen that the six elements contained in the Ti-Al-Cr-Nb-Si-Y high temperature oxidation resistant coating are 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0. 1Y 0.01 The types of elements in the multi-element alloy target remain consistent.

[0034] Figure 2 The surface SEM morphology of the Ti-Al-Cr-Nb-Si-Y high temperature oxidation resistant coating prepared in this example is shown in Figure 2. Figure 2 It can be seen that the structure of the Ti-Al-Cr-Nb-Si-Y high temperature anti-oxidation coating is dense and uniform.

[0035] Example 2

[0036] This embodiment includes the following steps:

[0037] Step 1, prefabrication of TiAl alloy substrate: using a machining center to perform precision milling and finishing on the surface of the TiAl alloy, and then polishing, and then cleaning until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying to obtain a prefabricated TiAl alloy substrate; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil and clean, and then use deionized water and ethanol solution in turn at 25°C to 40°C for 20 minutes respectively;

[0038] Step 2: Preparation of multi-element alloy target: Prepare Ti 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0.1 Y 0.01 The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment;

[0039] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0.1 Y 0.01 The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 -3 Pa, turn on the high-frequency plasma power supply, control the plasma voltage to 400V, then introduce H2 to adjust the pressure in the vacuum chamber to 1Pa, control the temperature of the vacuum chamber to 300°C, then apply a 40V base bias to the prefabricated TiAl alloy substrate, and use the formed electric field to perform plasma etching on the TiAl alloy substrate for 10min to remove oxide impurities on its surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 1Pa, and use a 200V base bias to perform plasma etching on the TiAl alloy substrate for 30min;

[0040] Step 4, multi-element coating deposition: apply an external electric field to -200 V to the TiAl alloy after Ar gas plasma etching in step 3, introduce argon gas into the vacuum chamber to adjust the vacuum degree to 1 Pa, and then start the cathode target arc for multi-arc ion plating. The cathode arc current is 100 A, and the temperature of multi-arc ion plating is maintained at 200°C for 20 minutes to obtain a TiAl alloy with a surface deposited Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating.

[0041] Example 3

[0042] This embodiment includes the following steps:

[0043] Step 1, prefabrication of TiAl alloy substrate: using a machining center to perform precision milling and finishing on the surface of the TiAl alloy, and then polishing, and then cleaning until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying to obtain a prefabricated TiAl alloy substrate; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil and clean, and then use deionized water and ethanol solution in turn at 25°C to 40°C for 15 minutes respectively;

[0044] Step 2: Preparation of multi-element alloy target: Prepare Ti 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0.1 Y 0.01 The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment;

[0045] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. 0.1 Al 0.6 Cr 0.16 Nb 0.03 Si 0.1 Y 0.01 The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 -3 Pa, turn on the high-frequency plasma power supply, control the plasma voltage to 300V, then introduce H2 to adjust the pressure in the vacuum chamber to 0.5Pa, control the temperature of the vacuum chamber to 300°C, then apply a 50V base bias to the prefabricated TiAl alloy substrate, and use the formed electric field to perform plasma etching on the TiAl alloy substrate for 10min to remove oxide impurities on its surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 0.5Pa, and use a 600V base bias to perform plasma etching on the TiAl alloy substrate for 30min;

[0046] Step 4, multi-element coating deposition: apply an external electric field to -100 V to the TiAl alloy after Ar gas plasma etching in step 3, introduce argon gas into the vacuum chamber to adjust the vacuum degree to 2 Pa, and then start the cathode target arc for multi-arc ion plating. The cathode arc current is 120 A, and the temperature of multi-arc ion plating is maintained at 400°C for 80 minutes to obtain a TiAl alloy with a surface deposited Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating.

[0047] Example 4

[0048] This embodiment includes the following steps:

[0049] Step 1, prefabrication of TiAl alloy substrate: using a machining center to perform precision milling and finishing on the surface of the TiAl alloy, and then polishing, and then cleaning until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying to obtain a prefabricated TiAl alloy substrate; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil and clean, and then use deionized water and ethanol solution in turn at 25°C to 40°C for 15 minutes respectively;

[0050] Step 2: Preparation of multi-element alloy target: Prepare Ti 0.3 Al 0.5 Cr 0.1 Nb 0.04 Si 0.05 Y 0.01 The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment;

[0051] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. 0.3 Al 0.5 Cr 0.1 Nb 0.04 Si 0.05 Y 0.01 The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 -3 Pa, turn on the high-frequency plasma power supply, control the plasma voltage to 300V, then introduce H2 to adjust the pressure in the vacuum chamber to 2Pa, control the temperature of the vacuum chamber to 400°C, then apply a 50V base bias to the prefabricated TiAl alloy substrate, and use the formed electric field to perform plasma etching on the TiAl alloy substrate for 15min to remove oxide impurities on its surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 2Pa, and use a 300V base bias to perform plasma etching on the TiAl alloy substrate for 60min;

[0052] Step 4, multi-element coating deposition: apply an external electric field to -100 V to the TiAl alloy after Ar gas plasma etching in step 3, introduce argon gas into the vacuum chamber to adjust the vacuum degree to 2 Pa, and then start the cathode target arc for multi-arc ion plating. The cathode arc current is 120 A, and the temperature of multi-arc ion plating is maintained at 400°C for 30 minutes to obtain a TiAl alloy with a surface deposited Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating.

[0053] Example 5

[0054] This embodiment includes the following steps:

[0055] Step 1, prefabrication of TiAl alloy substrate: using a machining center to perform precision milling and finishing on the surface of the TiAl alloy, and then polishing, and then cleaning until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying to obtain a prefabricated TiAl alloy substrate; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil and clean, and then use deionized water and ethanol solution in turn at 25°C to 40°C for 15 minutes respectively;

[0056] Step 2: Preparation of multi-element alloy target: Prepare Ti 0.3 Al 0.5 Cr 0.1 Nb 0.04 Si 0.05 Y 0.01 The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment;

[0057] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. 0.3 Al 0.5 Cr 0.1 Nb 0.04 Si 0.05 Y 0.01 The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 -3 Pa, turn on the high-frequency plasma power supply, control the plasma voltage to 300V, then introduce H2 to adjust the pressure in the vacuum chamber to 2Pa, control the temperature of the vacuum chamber to 300°C, then apply a 60V base bias to the prefabricated TiAl alloy substrate, and use the formed electric field to perform plasma etching on the TiAl alloy substrate for 20min to remove oxide impurities on its surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 2Pa, and use a 500V base bias to perform plasma etching on the TiAl alloy substrate for 30min;

[0058] Step 4, multi-element coating deposition: apply an external electric field to -200 V to the TiAl alloy after Ar gas plasma etching in step 3, introduce argon gas into the vacuum chamber to adjust the vacuum degree to 1.5 Pa, and then start the cathode target arc for multi-arc ion plating. The cathode arc current is 100 A, and the temperature of multi-arc ion plating is maintained at 400°C for 60 minutes to obtain a TiAl alloy with a surface deposited Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating.

[0059] Example 6

[0060] This embodiment includes the following steps:

[0061] Step 1, prefabrication of TiAl alloy substrate: using a machining center to perform precision milling and finishing on the surface of the TiAl alloy, and then polishing, and then cleaning until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying to obtain a prefabricated TiAl alloy substrate; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil and clean, and then use deionized water and ethanol solution in turn at 25°C to 40°C for 15 minutes respectively;

[0062] Step 2: Preparation of multi-element alloy target: Prepare Ti 0.3 Al 0.5 Cr 0.1 Nb 0.04 Si 0.05 Y 0.01 The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment;

[0063] Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. 0.3 Al 0.5 Cr 0.1 Nb 0.04 Si 0.05 Y 0.01 The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 -3 Pa, turn on the high-frequency plasma power supply, control the plasma voltage to 500V, then introduce H2 to adjust the pressure in the vacuum chamber to 1Pa, control the temperature of the vacuum chamber to 400°C, then apply a 60V base bias to the prefabricated TiAl alloy substrate, and use the formed electric field to perform plasma etching on the TiAl alloy substrate for 20min to remove oxide impurities on the surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 1Pa, and use a 500V base bias to perform plasma etching on the TiAl alloy substrate for 60min;

[0064] Step 4, multi-element coating deposition: apply an external electric field to -300 V to the TiAl alloy after Ar gas plasma etching in step 3, introduce argon gas into the vacuum chamber to adjust the vacuum degree to 1.5 Pa, and then start the cathode target arc for multi-arc ion plating. The cathode arc current is 80 A, and the temperature of multi-arc ion plating is maintained at 400°C for 80 minutes to obtain a TiAl alloy with a surface deposited Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating.

[0065] Figure 3 The 600h constant temperature oxidation weight change curve of the TiAl alloy with Ti-Al-Cr-Nb-Si-Y high temperature oxidation resistant coating and the TiAl alloy without coating prepared in Examples 5 to 6 of the present invention is shown in FIG. Figure 3It can be seen that compared with the TiAl alloy without deposited coating, the weight growth rate of the TiAl alloy with surface deposited Ti-Al-Cr-Nb-Si-Y high temperature anti-oxidation coating prepared in Example 5 is reduced by 76.75%, and the weight growth rate of the TiAl alloy with surface deposited Ti-Al-Cr-Nb-Si-Y high temperature anti-oxidation coating prepared in Example 6 is reduced by 61.88%, indicating that the Ti-Al-Cr-Nb-Si-Y high temperature anti-oxidation coating prepared in the present invention exhibits good high temperature anti-oxidation performance.

[0066] Figure 4 The macroscopic photographs of the substrate and the TiAl alloy with a Ti-Al-Cr-Nb-Si-Y high temperature oxidation resistant coating deposited on the surface used in Example 6 of the present invention after high temperature oxidation for 600 hours, wherein Figure (a) represents the substrate TiAl alloy, and Figure (b) represents the TiAl alloy with a Ti-Al-Cr-Nb-Si-Y high temperature oxidation resistant coating deposited on the surface. Figure 4 It can be seen that the TiAl alloy with Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating deposited on the surface turns black after oxidation, but the coating surface is smooth and complete without any peeling or falling off. The base TiAl alloy without coating deposited is yellow in color, and the sample has severe peeling and falling off. The oxide layer produced during the high-temperature oxidation process has fallen off very seriously.

[0067] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high temperature anti-oxidation coating suitable for TiAl alloy, characterized in that: The method comprises the following steps: Step 1: Prefabrication of TiAl alloy substrate: After finishing the surface of the TiAl alloy, polishing treatment is performed, and then cleaning is performed until there is no dust, oil stains, water stains and other impurities on the surface, and then washing and drying is performed to obtain a prefabricated TiAl alloy substrate; Step 2: Preparation of multi-element alloy target: Prepare Ti a Al b Cr c Nb d Si e Y f The multi-element alloy target is installed on the cathode target position of the vacuum chamber of the multi-arc ion plating equipment, wherein a, b, c, d, e, and f represent the atomic proportions of the corresponding elements, and a+b+c+d+e+f=1, 0.1≤a≤0.3, 0.5≤b≤0.6, 0.1≤c≤0.16, 0.03≤d≤0.04, 0.05≤e≤0.10, and f≈0.01; Step 3: Etching the substrate: Place the TiAl alloy substrate prepared in step 1 on the substrate containing Ti prepared in step 2. a Al b Cr c Nb d Si e Y f The multi-element alloy target is placed on the vacuum chamber carrier, and the vacuum chamber pressure is evacuated to a value not exceeding 5×10 - 3 Pa, turn on the high-frequency plasma power supply, then introduce H2 to adjust the pressure in the vacuum chamber to 0.5Pa~2Pa, then apply bias to the prefabricated TiAl alloy substrate, and the formed electric field performs plasma etching on the TiAl alloy substrate to remove oxide impurities on the surface, then stop introducing H2, introduce Ar gas to adjust the pressure in the vacuum chamber to 0.5Pa~2Pa, and continue to perform plasma etching on the TiAl alloy substrate; Step 4: multi-element coating deposition: an external electric field is applied to the TiAl alloy after Ar gas plasma etching in step 3, and argon gas is introduced into the vacuum chamber to adjust the vacuum degree, and then the cathode target arc is started for multi-arc ion plating to obtain a TiAl alloy with a Ti-Al-Cr-Nb-Si-Y high-temperature anti-oxidation coating deposited on the surface.

2. The method for preparing a high temperature oxidation resistant coating suitable for TiAl alloy according to claim 1, characterized in that: The finishing process described in step 1 is to use a machining center to perform precision milling on the TiAl alloy surface.

3. The method for preparing a high temperature oxidation resistant coating suitable for TiAl alloy according to claim 1, characterized in that: The cleaning process in step 1 is: first use an industrial degreasing cleaning agent for degreasing cleaning, and then use deionized water and ethanol solution in turn for ultrasonic cleaning at 25° C. to 40° C. for 15 min to 20 min respectively.

4. The method for preparing a high temperature anti-oxidation coating suitable for TiAl alloy according to claim 1, characterized in that: In step three, turn on the high-frequency plasma power supply to control the plasma voltage to 200V~500V, the vacuum chamber temperature to 200℃~400℃, the substrate bias voltage to 40V~60V when H2 is introduced for plasma etching, and the etching time is 10min, and the substrate bias voltage to 200V~600V when Ar gas is introduced for plasma etching, and the etching time is 30min~60min.

5. The method for preparing a high temperature anti-oxidation coating suitable for TiAl alloy according to claim 1, characterized in that: The voltage of the applied electric field in step 4 is -100V to -350V, the vacuum degree is adjusted to 0.5Pa to 2Pa, the cathode arc current generated by the cathode target arc is 50A to 120A, the temperature of the multi-arc ion plating is maintained at 150°C to 400°C, and the time is 20min to 80min.

6. A high temperature oxidation resistant coating suitable for TiAl alloy, characterized in that: The method is prepared by any one of claims 1 to 5.

Citation Information

Patent Citations

  • Titanium alloy surface ceramic / metal gradient high-temperature composite coating and preparing method thereof

    CN105714244A

  • TiAl coating capable of achieving heat growth of aluminum oxide film and preparing method of TiAl coating

    CN105908131A

  • Method for preparing TiAlSiCN coating by ion plating

    CN106591784A

  • A NiCrAlSi / CeO2 doped YSZ coating on the surface of a gamma-TiAl alloy and a preparing method thereof

    CN109207939A

  • Method for improving high-temperature oxidation resistance of Ti-45Al-8.5Nb alloy

    CN109536883A

Cited By

  • Titanium-aluminum alloy blade high-temperature coating homogenizing deposition method based on profiling fastening clamp

    CN120738610A

  • Titanium-aluminum alloy blade high-temperature coating homogenization deposition method based on a profiling fastening clamp