Porous low-loss oxygen evolution electrode and preparation method thereof

By optimizing the porous structure and electronic structure of the electrode material, and combining it with citric acid to build a three-dimensional network, the problem of low catalytic activity and poor stability of the oxygen evolution electrode is solved, and high-efficiency, low-loss oxygen evolution performance and long-life electrode materials are achieved. in PEM electrolysis system.

CN118727031APending Publication Date: 2024-10-01HANGZHOU CHANGHYDROGEN NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410745828.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing oxygen evolution electrodes have low catalytic activity, easy separation of active materials from the substrate, high preparation costs, and poor long-term stability. Especially in PEM electrolysis systems, their effects are limited.

Method used

By using divinylbenzene, styrene, toluene and other materials for suspension prepolymerization, polymerization and heat treatment, porous carbon-based electrode materials are formed, and the electronic structure is optimized through metal components such as Ni, Fe, Co, Mo, Cu, etc., combined with lemon The acid constructs a three-dimensional network structure to improve the catalytic activity and stability of the electrode.

Benefits of technology

It achieves efficient oxygen evolution performance, extends the service life of electrode materials, reduces preparation costs, and shows good stability and efficiency in the PEM electrolysis system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004886410360000061
    Figure BDA0004886410360000061
  • Figure BDA0004886410360000072
    Figure BDA0004886410360000072
  • Figure BDA0004886410360000081
    Figure BDA0004886410360000081
Patent Text Reader

Abstract

The invention belongs to the field of electrode materials, and particularly relates to a porous low-loss oxygen evolution electrode and a preparation method thereof. The method comprises the following steps: 1) taking organic matters, uniformly mixing, adding excessive calcium salt aqueous solution, carrying out suspension prepolymerization and polymerization, and carrying out drying, preoxidation and heat treatment to obtain a carbon-based material; 2) uniformly mixing metal nitrate and an organic solvent to obtain a liquid phase A, uniformly mixing metal oxide acid salt and water to obtain a liquid phase B, adding organic acid to react while mixing the liquid phase A, the liquid phase B and the carbon-based material, and drying to obtain a composite material; 3, the composite material is taken to be subjected to heat treatment, and the oxygen evolution electrode is obtained.Active substances on the prepared oxygen evolution electrode are evenly distributed, the oxygen evolution electrode has good oxygen evolution performance and long service life, and the problem that bubbles form an air cushion, so that active sites are shielded can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrode materials, and in particular relates to a porous low-loss oxygen evolution electrode and a preparation method thereof. Background Art

[0002] The production of hydrogen and oxygen by decomposing water is an important energy conversion method, and the electrolysis of water is an important method for producing high-purity hydrogen and high-purity oxygen. In order to promote the oxygen evolution process, it is important to find an efficient and suitable electrolysis system. The theoretical decomposition voltage of water is independent of the pH value. From the perspective of the structure of the electrolyzer and the selection of materials, the use of acidic electrolytes is prone to cause electrolyzer failures, so alkaline solutions are used in industry. However, with the in-depth study of the corresponding electrolysis technology, it is found that the PEM electrolysis process is technically higher than the traditional alkaline water electrolysis process, and it has the characteristics of high efficiency, safety, pollution-free and high efficiency. In this regard, technicians in this field have conducted a series of studies and mainly found three types of materials: coated type, single atom type, and binder-free type. Among them, the coated electrode material is obtained by regulating the metal "core" component, regulating the thickness of the carbon shell, and modifying the element doping, which can improve the catalytic performance of the electrode material. However, most of the existing materials are irregular in shape. Since it is difficult to avoid particle agglomeration, the effective active area is significantly reduced compared to the theoretically calculated specific surface area, resulting in a low charge transfer rate. Although single-atom electrode materials can show high HER activity in acid-base systems, they are not effective in hydrogen and oxygen evolution when multi-metal sites are required for coordinated catalysis. They cannot completely replace coated electrode materials and have limited effects in PEM systems. Coated and single-atom electrode materials need to adhere to the electrode surface, and the bonding strength between the composite layer and the substrate needs to be considered. The electrode area limits the loading amount of active substances. Voltage needs to be applied during application, which significantly increases energy consumption and is not conducive to widespread application in industry. In addition, the energy and power density of binder-free electrode materials are significantly increased, but there are problems such as low bonding strength with the substrate and easy detachment of active substances, which cannot withstand long-term charge and discharge cycles.

[0003] Patent CN114000164A discloses a novel oxygen evolution electrode and a preparation method thereof, wherein the oxygen evolution electrode is composed of the following raw materials by weight: 1 to 60 parts of carbon nanotube particles, 1 to 50 parts of electrode solvent and 0.1 to 5 parts of electrode emulsion, wherein the carbon nanotube particles are loaded with 0.1 to 20 wt% of copper, iridium and ruthenium noble metal oxides, the electrode solvent includes any one of ethanol, isopropanol, n-butanol and n-propanol, and the electrode emulsion includes polytetrafluoroethylene emulsion or polyvinylidene fluoride emulsion. The carbon nanotube loaded with copper, iridium and ruthenium noble metal oxides is placed in a ball mill and ball milled at 300 to 1200 r / min for 5 to 30 minutes to obtain carbon nanotube particles; the electrode solvent and the electrode emulsion are added to the carbon nanotube particles at room temperature and stirred to obtain a mixture A; the mixture A is stirred at a temperature of 50 to 95°C to obtain a mass B; the mass B is rolled into a film and cut according to size. This oxygen evolution electrode can have good oxygen evolution performance, but its cost is too high and its service life is limited. It is not suitable for industrial applications and is difficult to be effectively applied to PEM electrolysis systems. Summary of the invention

[0004] Based on the above content, in order to solve the problems of low catalytic activity of oxygen evolution electrode, easy separation of active material from substrate, high preparation cost, poor long-term stability, etc., the present invention proposes a porous low-loss oxygen evolution electrode and a preparation method thereof.

[0005] The objects of the present invention are:

[0006] 1. Increase the loading amount of active substances;

[0007] 2. Ensure that the oxygen evolution electrode has good oxygen evolution performance;

[0008] 3. Extend the service life of electrode materials;

[0009] 4. It can be effectively applied to PEM electrolysis system.

[0010] To achieve the above objectives, the present invention adopts the following technical solutions.

[0011] A method for preparing a porous low-loss oxygen evolution electrode,

[0012] The method comprises:

[0013] 1) taking organic matter and mixing it evenly, adding an excess of calcium salt aqueous solution for suspension prepolymerization and polymerization, and obtaining a carbon-based material through drying, preoxidation and heat treatment;

[0014] 2) mixing a metal nitrate and an organic solvent to obtain a liquid phase A, mixing a metal oxide acid salt and water to obtain a liquid phase B, adding an organic acid to the mixture of the liquid phase A, the liquid phase B and the carbon-based material to react, and drying to obtain a composite material;

[0015] 3) The composite material is subjected to heat treatment, and then rapidly cooled, cleaned and dried to obtain an oxygen evolution electrode.

[0016] As a preference,

[0017] Step 1) The organic matter is divinylbenzene, styrene, or toluene;

[0018] The divinylbenzene, styrene and toluene are prepared in a volume ratio of (1-1.2):1:(0.4-0.6).

[0019] As a preference,

[0020] Step 1) The solute of the calcium salt aqueous solution is CaCl2, and its mass fraction is 1.2-1.8wt%.

[0021] As a preference,

[0022] The suspension prepolymerization in step 1) is carried out at a constant temperature of 50 to 60° C. for 10 to 15 minutes;

[0023] The polymerization in step 1) is carried out at a constant temperature of 80 to 90° C. for 7 to 8 hours;

[0024] Step 1) The pre-oxidation is carried out in an air atmosphere at a constant temperature of 300-350° C. for 4-5 hours;

[0025] Step 1) The heat treatment is carried out under an inert atmosphere at a constant temperature of 600-650° C. for 1-2 hours.

[0026] As a preference,

[0027] Step 2) the metal nitrate is a mixture of nickel nitrate hexahydrate, iron nitrate nonahydrate, cobalt nitrate hexahydrate and copper nitrate trihydrate;

[0028] The nickel nitrate hexahydrate, the iron nitrate nonahydrate, the cobalt nitrate hexahydrate, and the copper nitrate trihydrate are prepared in a mass ratio of (18-19.2):(6.7-8.3):(1.2-2.4):1;

[0029] Step 2) The organic solvent is ethanol, and its usage is 8-10 mL / g metal nitrate.

[0030] As a preference,

[0031] Step 2) the metal oxide acid salt is ammonium molybdate tetrahydrate, and its dosage is 1.5-2g / g metal nitrate;

[0032] The amount of water used in step 2) is 8-10 mL / g of metal oxide acid salt.

[0033] As a preference,

[0034] Step 2) The amount of the carbon-based material is 1.5-2 g / mL of the total volume of the mixture of liquid phase A and liquid phase B;

[0035] Step 2) The organic acid is citric acid, and its dosage is 0.3-0.4 g / g metal nitrate.

[0036] As a preference,

[0037] Step 2) The reaction is carried out at 80-90°C in a water bath for 0.5-1 h.

[0038] As a preference,

[0039] Step 3) The heat treatment is carried out at 600-700° C. for 4-5 hours.

[0040] A porous low-loss oxygen evolution electrode.

[0041] In the technical solution of the present invention, divinylbenzene and styrene are used as carbon sources, and toluene is used as a pore-forming agent to prepare a porous electrode substrate. However, the micropores of the electrode material that is only chemically cross-linked are of different sizes. Under the impact of current, it will still cause a large energy loss and unstable oxygen evolution performance. The present invention utilizes the difference in hydration properties of polymers and salts to regulate the ratio of free water and bound water in the polymerization system and constrain the polymer molecular chain. And with the increase in the amount of CaCl2 salt, the distance between the molecular chains decreases, that is, the spatial constraint successfully makes the molecular chains closer, and the stability of the electrode substrate is enhanced. After characterization, it was found that the carbon-based electrode is a lamellar structure with abundant mesopores. Based on the abundant capillary effect, the smaller the pores, the greater the influence of the electrolyte affinity of the material. However, if the amount of toluene is too little or not used, the pores of the substrate are too small. Due to the influence of capillary tension, the electrolyte affinity of the material is extremely poor at this time, so the electrolyte cannot transfer mass well. If too large pores are formed, although the material has good electrolyte affinity and the electrolyte can transfer mass quickly and smoothly, the electrolyte ions can enter the pores larger than the radius of the hydrated ions, thereby storing energy.

[0042] In order to improve the catalytic performance of the electrode material, the present invention increases the number and reactivity of active sites by optimizing the electronic structure. High entropy alloys have adjustable electronic structures, optimizable d-band centers and excellent structural stability, which can bring higher adsorption strength and maximize the catalytic activity of the electrode. Therefore, the present invention optimizes the electronic structure of the electrode through five metal components, namely Ni, Fe, Co, Mo and Cu, taking into account both faster charge transfer rate and better structural stability. With the increase of nickel dosage, the B2 structure in the alloy is transformed into an FCC structure, the hardness of the electrode material is increased, and it is not easy to break under large current impact, which prolongs the service life. The Fe component can significantly improve the performance of the co-based electrocatalyst. After Fe doping and in-situ electro-oxidation, more active sites are generated, which accelerates the diffusion of electrolytes and the transfer of electrons, and can buffer the volume changes caused by oxygen evolution. Co can promote the uniform distribution of metals other than Cu. In addition, a small amount of Mo element can improve the problem of metal segregation, so that the high entropy alloy produces an ordered strengthening phase, promotes the precipitation of σ phase, inhibits the generation of defects, and further improves the hardness and strength of the electrode material. However, since the atomic radius of Mo is significantly larger than that of other atoms, if excessive Mo is added, it will cause serious lattice distortion of atoms during diffusion, which will cause the electrode material to break easily under high current impact. In addition, the ratio of Ni, Fe and Co has a great influence on the corrosion resistance of the alloy. Considering the preparation cost and the above reasons, the present invention strictly controls the amount of metal.

[0043] Ni, Fe, Co, Mo, and Cu are adjacent transition metal elements with similar atomic radius, electronegativity, and mixing enthalpy. They are easy to alloy. Metal nitrates and ammonium molybdate dissolve to produce orthomolybdate, nitrate, and transition metal ions. When the transition metal ions are complexed with citric acid, they are mixed, heat treated, and dehydrated to form a three-dimensional network structure by cross-linking and polycondensation with citric acid. The high entropy alloy layer and the carbon-based material are successfully composited with high bonding strength. After heat treatment, the alloy will precipitate a precipitate phase rich in Ni, Co, and Mo elements. The alloy has a dense structure and higher microhardness, which can extend the service life of the electrode material. The present invention regulates Cu by changing the amount of citric acid used. 2+The coordination mode of plasma and carboxylic acid, ions with strong coordination ability participate in the construction of a three-dimensional network skeleton, while ions with weak coordination ability are in a free state, which makes the active material grain size differentiated. According to research in this field, when a large number of carboxylates are coordinated with metal ions in a monodentate or bridge form, it is conducive to the formation of a three-dimensional network structure with metal ions as nodes. Citric acid as a complexing agent can ensure the uniformity of raw material components and higher product purity. With the increase of citric acid dosage, due to the electron-withdrawing effect of metal ions, the electrons on OH are offset to the metal ions and the bond strength increases, the structure is more stable, and the grain size of the electrode surface active material becomes smaller, which is conducive to improving the electrocatalytic activity of the electrode. However, if excessive citric acid is used, the coordination form between citric acid and metal ions is changed from monodentate coordination to bidentate bridge coordination and multidentate coordination. The excessive multidentate coordination structure causes the electrode surface active material grain size to be too small, the surface energy becomes larger, and serious agglomeration occurs.

[0044] After characterization, it was found that the metal active sites in the present invention have strong adsorption activity, promoting H + According to research in this field, it is found that multiple alloying of the electrode substrate alone can also improve the catalytic activity of the electrode material, but the improvement effect has not reached the expected level. The reason is that high entropy alloys are single-phase solid solutions, and the elements work together to promote the hydrogen and oxygen evolution reactions. For example, when a single pure nickel powder is used to composite carbon-based materials, H + The desorption reaction barrier is higher, the reaction is hindered, and the oxygen evolution amount is lower.

[0045] At the same time, under the condition of high current density, a large number of bubbles will be generated on the electrode surface. When the bubbles gather and adhere to the active sites of the electrode material, an air cushion is formed, which causes the active sites to be "shielded," making it difficult for the electrolyte to diffuse, and the oxygen evolution rate is significantly reduced. Large bubbles have a greater adhesion to the electrode material and may peel off the active substance. Therefore, the present invention enhances the stability of the material by regulating the composition of the electrode material and the active substance, and constructs a hydrophilic and gas-repellent electrode surface by regulating the morphology of the surface of the active substance. By regulating the roughness of the solid-liquid-gas three-phase contact interface, the electrode material prepared by the present invention can divide large bubbles into discontinuous small bubbles, that is, avoid the generation of excessively large bubbles, reduce the contact area between the bubbles and the electrode material, and achieve rapid desorption of bubbles. After the rapid desorption of the bubbles, the active sites are exposed again, and the mass transfer of the electrolyte is promoted. After characterization and experiments, it is found that the surface roughness of the oxygen evolution electrode prepared by the present invention is large, showing good oxygen evolution performance, and has good oxygen evolution stability when used.

[0046] The beneficial effects of the present invention are as follows:

[0047] (1) The active material on the oxygen evolution electrode prepared by the present invention is evenly distributed, and has good oxygen evolution performance;

[0048] (2) The oxygen evolution electrode prepared by the present invention has a long service life;

[0049] (3) The oxygen evolution electrode prepared by the present invention can avoid the problem of bubbles forming an air cushion, thereby causing the active sites to be "shielded". DETAILED DESCRIPTION

[0050] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0051] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0052] Unless otherwise specified, the composite material prepared in the embodiment of the present invention is pressed into a specification of 1 mm in thickness and 5 cm×2 cm in front and back.

[0053] Example 1

[0054] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0055] 1) Take 3mL of divinylbenzene, 3mL of styrene, and 1.2mL of toluene and mix them evenly, add 20mL of a CaCl2 aqueous solution with a mass fraction of 1.2wt%, keep the temperature at 50°C for 15min, and then keep the temperature at 80°C for 8h. After drying, keep the temperature at 300°C for 5h in an air atmosphere and keep the temperature at 600°C for 2h in a N2 atmosphere to obtain a carbon-based material; 2) Take 1.8g of nickel nitrate hexahydrate, 0.68g of iron nitrate nonahydrate, 0.12g of cobalt nitrate hexahydrate, 0.1g of copper nitrate trihydrate, and 25mL of ethanol and mix them evenly to obtain liquid phase A, take 4.1g of ammonium molybdate tetrahydrate, and 35mL of water and mix them evenly to obtain liquid phase B, mix liquid phase A and liquid phase B, add 90g of carbon-based material and 0.81g of citric acid, and water bath at 90°C for 0.5h to obtain a composite material after drying;

[0056] 3) The composite material is placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The performance of the oxygen evolution electrode prepared in this example is tested in the following manner.

[0057] 1. Hardness test:

[0058] Five areas of the electrode sample were taken for Vickers hardness testing.

[0059] 2. Electrochemical test:

[0060] Using 1 mol / L KOH solution as electrolyte, the oxygen evolution electrode prepared by the present invention as working electrode, a nickel-based electrode as counter electrode, a saturated calomel electrode as reference electrode, iR correction at a scanning rate of 2.0 mV / s, electrochemical test was carried out, and the Tafel slope was calculated according to the current density and overpotential.

[0061] 3. Cyclic test:

[0062] Chronopotentiometry was used at 50 mA / cm 2 A 72-hour continuous stability test is conducted at the current density. If there is no obvious loss of electrode material (loss rate ≤ 0.5‰) and no significant decrease in oxygen evolution performance (oxygen evolution performance decrease rate ≤ 1.0‰), it is recorded as "PASS." If there is obvious stratification or detachment of the electrode material or a significant decrease in oxygen evolution performance, it is recorded as "FAIL."

[0063] 4. Oxygen evolution activity:

[0064] The oxygen evolution electrode in this example is used as the anode (working electrode), the conventional platinum carbon active electrode is used as the counter electrode (cathode), and a conventional water electrolysis system is assembled (pure water is used as the oxygen production electrolyte raw material, and the solid polymer membrane is used as the electrolytic membrane). During the water electrolysis process, the constant current density is controlled to be 1.2A / cm 2 , measure the oxygen production of the working electrode per hour when electrolyzing water, and calculate the oxygen production rate.

[0065] The results are as follows.

[0066]

[0067]

[0068] According to the results in the above table, the oxygen evolution material of the present invention has a faster oxygen production rate. According to the indentation load-displacement curve, it can be measured that under the condition of a load of 20mN, the indentation depth of the electrode material is 0.1μm. Combined with the Vickers hardness of the electrode material, it can be analyzed that compared with pure carbon-based materials, the hardness of the electrode material prepared by the present invention is enhanced. Under high current density, there is no obvious loss in the electrode material, and there is no obvious fluctuation in the test curve, which shows that the electrode material prepared by the present invention has a good service life and has good application prospects. When the current density is increased from 50mA / cm 3 Change to 100mA / cm 3When the overpotential is only 358mV and 373mV, it shows a low oxygen evolution overpotential, indicating that the electrode material prepared by the present invention has good catalytic activity. At the same time, the oxygen production rate is better and the cyclic performance is very excellent. In particular, conventional oxygen evolution electrodes, under continuous working conditions, often have a decrease in oxygen evolution performance within 72 hours after bubbles are attached to the surface, and the maximum decrease can even reach more than 15%. The oxygen evolution electrode of the present invention shows extremely excellent degassing, which suppresses the decrease rate of its oxygen evolution performance to an extremely low level, and can even be controlled within 1‰ within 72 hours.

[0069] Example 2

[0070] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0071] 1) Take 3mL of divinylbenzene, 3mL of styrene, and 1.2mL of toluene and mix them evenly, add 20mL of a CaCl2 aqueous solution with a mass fraction of 1.2wt%, keep the temperature at 50°C for 15min, and then keep the temperature at 80°C for 8h. After drying, keep the temperature at 300°C for 5h in an air atmosphere and keep the temperature at 600°C for 2h in a N2 atmosphere to obtain a carbon-based material; 2) Take 1.8g of nickel nitrate hexahydrate, 0.68g of iron nitrate nonahydrate, 0.12g of cobalt nitrate hexahydrate, 0.1g of copper nitrate trihydrate, and 25mL of ethanol and mix them evenly to obtain liquid phase A, take 4.1g of ammonium molybdate tetrahydrate, and 35mL of water and mix them evenly to obtain liquid phase B, mix liquid phase A and liquid phase B, add 90g of carbon-based material and 0.95g of citric acid, and water bath at 90°C for 0.5h to obtain a composite material after drying;

[0072] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The performance test of the oxygen evolution electrode prepared in this example was carried out in the same manner as in Example 1, and the results were as follows.

[0073]

[0074] Citric acid as a complexing agent can ensure the uniformity of raw material components, higher product purity, and regulate the ions with strong coordination ability to participate in the construction of a three-dimensional network skeleton, while the ions with weaker coordination ability are in a free state, so that the active material grain size is differentiated. According to the results in the table of Examples 1 to 2, due to the electron-withdrawing effect of metal ions, as the amount of citric acid increases, the electrons on OH shift toward the metal ions and the bond strength increases, the structure is more stable, and the grain size of the active material on the electrode surface becomes smaller, the electrocatalytic activity of the electrode is improved, and the oxygen production rate is increased. According to the further decrease in overpotential and Tafel slope, it can be analyzed that the charge transfer rate is accelerated, and the material in this example still maintains good stability.

[0075] Example 3

[0076] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0077] 1) 3 mL of divinylbenzene, 3 mL of styrene, and 1.2 mL of toluene were mixed uniformly, 20 mL of a 1.2 wt% CaCl2 aqueous solution was added, and the mixture was kept at a constant temperature of 50°C for 15 min, and then kept at a constant temperature of 80°C for 8 h. After drying, the mixture was kept at a constant temperature of 300°C for 5 h in an air atmosphere, and kept at a constant temperature of 600°C for 2 h in a N2 atmosphere to obtain a carbon-based material; 2) 1.8 g of nickel nitrate hexahydrate, 0.68 g of iron nitrate nonahydrate, 0.12 g of cobalt nitrate hexahydrate, 0.1 g of copper nitrate trihydrate, and 25 mL of ethanol were mixed uniformly to obtain a liquid phase A, 4.1 g of ammonium molybdate tetrahydrate and 35 mL of water were mixed uniformly to obtain a liquid phase B, the mixed liquid phases A and B were added, 90 g of the carbon-based material was added, and 1.08 g of citric acid was added at the same time, and the mixture was kept in a water bath at 90°C for 0.5 h, and the composite material was obtained after drying;

[0078] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The oxygen evolution electrode prepared in this example was tested for performance in the same manner as in Example 1, and the results were as follows.

[0079]

[0080] According to technical research in this area, it is found that when a large number of carboxylates are coordinated with metal ions in a monodentate or bridge form, it is conducive to the formation of a three-dimensional network structure with metal ions as nodes. In this case, a large amount of citric acid is coordinated with metal ions, which promotes the coordination form between metal ions from monodentate coordination to bidentate bridge coordination and multidentate coordination. The grain size of the active material on the electrode surface is getting smaller and smaller, the surface energy is getting larger and larger, and local agglomeration occurs. Therefore, the oxygen evolution of the material decreases slightly, resulting in a decrease in the average oxygen production rate. According to the results in the above table, the Tafel slope becomes larger, indicating that the current increases, the voltage increases to a large extent, and the energy consumption required for oxygen evolution is large. This conclusion can be consistent with the result of the decrease in the average oxygen production rate.

[0081] In summary, the oxygen evolution electrode prepared by the present invention has good oxygen evolution performance and shows high stability. After continuous use for 75 hours, the current density does not decay significantly, and the LCV curve does not change after 1000 cycles, indicating that the oxygen evolution electrode prepared by the present invention has good application prospects.

[0082] Comparative Example 1

[0083] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0084] 1) 3 mL of divinylbenzene, 3 mL of styrene, and 0.8 mL of toluene were mixed uniformly, 20 mL of a CaCl2 aqueous solution with a mass fraction of 1.2 wt% was added, and the mixture was kept at a constant temperature of 50°C for 15 min, and then kept at a constant temperature of 80°C for 8 h. After drying, the mixture was kept at a constant temperature of 300°C for 5 h in an air atmosphere, and at a constant temperature of 600°C for 2 h in a N2 atmosphere to obtain a carbon-based material; 2) 1.8 g of nickel nitrate hexahydrate, 0.68 g of ferric nitrate nonahydrate, 0.12 g of cobalt nitrate hexahydrate, 0.1 g of copper nitrate trihydrate, and 25 mL of ethanol were mixed uniformly to obtain a liquid phase A, 4.1 g of ammonium molybdate tetrahydrate and 35 mL of water were mixed uniformly to obtain a liquid phase B, the mixed liquid phases A and B were added, 90 g of the carbon-based material was added, and 0.95 g of citric acid was added at the same time, and the mixture was kept in a water bath at 90°C for 0.5 h, and the composite material was obtained after drying;

[0085] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The oxygen evolution electrode prepared in this example was tested for performance in the same manner as in Example 1, and the results were as follows.

[0086]

[0087] In this case, the amount of toluene used was too small. After characterization, it was found that the pore diameter of the material became smaller. Due to the influence of capillary tension, its electrolyte affinity became worse, so the electrolyte could not transfer mass well, thereby reducing the oxygen production rate of the material.

[0088] In addition, if 2mL toluene is used instead, larger pores will be formed. Although the material has good electrolyte affinity at this time and the electrolyte can transfer mass quickly and smoothly, the electrolyte ions can enter the pores that are larger than the radius of the hydrated ions, thereby storing energy. This still affects the oxygen evolution performance of the material. At the same time, under the impact of current, the electrode material is not stable enough, which will cause a large energy loss.

[0089] Comparative Example 2

[0090] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0091] 1) 3 mL of divinylbenzene, 3 mL of styrene and 1.2 mL of toluene were mixed and kept at 50° C. for 15 min, then kept at 80° C. for 8 h, dried, kept at 300° C. for 5 h in air atmosphere, and kept at 600° C. for 2 h in N2 atmosphere to obtain a carbon-based material;

[0092] 2) 1.8 g of nickel nitrate hexahydrate, 0.68 g of iron nitrate nonahydrate, 0.12 g of cobalt nitrate hexahydrate, 0.1 g of copper nitrate trihydrate, and 25 mL of ethanol were mixed to obtain liquid phase A, 4.1 g of ammonium molybdate tetrahydrate and 35 mL of water were mixed to obtain liquid phase B, liquid phase A and liquid phase B were mixed, 90 g of carbon-based material and 0.95 g of citric acid were added, and the mixture was incubated at 90° C. in a water bath for 0.5 h, and dried to obtain a composite material;

[0093] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The performance test of the oxygen evolution electrode prepared in this example was carried out in the same manner as in Example 1, and the results were as follows.

[0094]

[0095] Since CaCl2 plays a role in reducing the distance between molecular chains and constraining molecular chains, the hardness of the electrode material without CaCl2 component in this example is significantly reduced. Under the impact of current, the material is damaged, which seriously affects the oxygen evolution performance.

[0096] Comparative Example 3

[0097] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0098] 1) 3 mL of divinylbenzene, 3 mL of styrene, and 1.2 mL of toluene were mixed uniformly, 20 mL of a 1.2 wt% CaCl2 aqueous solution was added, and the mixture was kept at a constant temperature of 50°C for 15 min, and then kept at a constant temperature of 80°C for 8 h. After drying, the mixture was kept at a constant temperature of 300°C for 5 h in an air atmosphere, and at a constant temperature of 600°C for 2 h in a N2 atmosphere to obtain a carbon-based material; 2) 2.0 g of nickel nitrate hexahydrate, 0.68 g of ferric nitrate nonahydrate, 0.12 g of cobalt nitrate hexahydrate, 0.1 g of copper nitrate trihydrate, and 25 mL of ethanol were mixed uniformly to obtain a liquid phase A, 4.1 g of ammonium molybdate tetrahydrate and 35 mL of water were mixed uniformly to obtain a liquid phase B, the mixed liquid phases A and B were added, 90 g of the carbon-based material was added, and 0.95 g of citric acid was added at the same time, and the mixture was kept in a water bath at 90°C for 0.5 h, and the composite material was obtained after drying;

[0099] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The performance test of the oxygen evolution electrode prepared in this example was carried out in the same manner as in Example 1, and the results were as follows.

[0100]

[0101] In this case, the electrode material changes from a BCC+B2 structure to a BCC+FCC structure. On the one hand, nickel salt is beneficial to the growth of active sites, but on the other hand, excessive nickel salt only leads to an increase in the proportion of the FCC phase, which makes the electrode material brittle and affects the oxygen evolution performance.

[0102] Comparative Example 4

[0103] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0104] 1) Take 3mL of divinylbenzene, 3mL of styrene, and 1.2mL of toluene and mix them evenly, add 20mL of a CaCl2 aqueous solution with a mass fraction of 1.2wt%, keep the temperature at 50°C for 15min, and then keep the temperature at 80°C for 8h. After drying, keep the temperature at 300°C for 5h in an air atmosphere and keep the temperature at 600°C for 2h in a N2 atmosphere to obtain a carbon-based material; 2) Take 1.8g of nickel nitrate hexahydrate, 0.12g of cobalt nitrate hexahydrate, 0.78g of copper nitrate trihydrate, and 25mL of ethanol and mix them evenly to obtain liquid phase A, take 4.1g of ammonium molybdate tetrahydrate, and 35mL of water and mix them evenly to obtain liquid phase B, mix liquid phase A and liquid phase B, add 90g of carbon-based material and 0.95g of citric acid, and water bath at 90°C for 0.5h to obtain a composite material after drying;

[0105] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The oxygen evolution electrode prepared in this example was tested for performance in the same manner as in Example 1, and the results were as follows.

[0106]

[0107] In this example, the composite components are replaced in equal amounts, which not only causes the catalytic performance of the electrode material to decrease, but also causes the material to fall off after power is applied. According to technical research in this field, after Fe doping and in-situ electro-oxidation, there are more active sites on the electrode material, which can accelerate the diffusion of electrolytes and the transfer of electrons, and on the other hand, can buffer the volume change caused by oxygen evolution. Therefore, the structural stability of the electrode material in this example is insufficient. Moreover, the advantage of the present invention using five adjacent transition metal elements Ni, Fe, Co, Mo, and Cu to synthesize high entropy alloys is that the alloy is single-phase solid solution after heat treatment, and its components are uniformly dense, which can improve the hardness of the material and ensure the service life of the electrode material. At the same time, each element synergizes and promotes the hydrogen evolution and oxygen evolution reactions together. In this example, only a simple multiple alloying of the electrode substrate is performed, which is not enough to improve the substrate effect.

[0108] Comparative Example 5

[0109] A method for preparing a porous low-loss oxygen evolution electrode, the method comprising:

[0110] 1) Take 3mL of divinylbenzene, 3mL of styrene, and 1.2mL of toluene and mix them evenly, add 20mL of a CaCl2 aqueous solution with a mass fraction of 1.2wt%, keep the temperature at 50°C for 15min, and then keep the temperature at 80°C for 8h. After drying, keep the temperature at 300°C for 5h in an air atmosphere and keep the temperature at 600°C for 2h in a N2 atmosphere to obtain a carbon-based material; 2) Take 1.8g of nickel nitrate hexahydrate, 0.68g of iron nitrate nonahydrate, 0.12g of cobalt nitrate hexahydrate, 0.1g of copper nitrate trihydrate, and 25mL of ethanol and mix them evenly to obtain liquid phase A, take 5.8g of ammonium molybdate tetrahydrate, and 35mL of water and mix them evenly to obtain liquid phase B, mix liquid phase A and liquid phase B, add 90g of carbon-based material and 0.95g of citric acid, and water bath at 90°C for 0.5h to obtain a composite material after drying;

[0111] 3) The composite material was placed at 600°C for 5 hours, cooled rapidly, and washed and dried to obtain an oxygen evolution electrode. The oxygen evolution electrode prepared in this example was tested for performance in the same manner as in Example 1, and the results were as follows.

[0112]

[0113] Co can promote the uniform distribution of metals other than Cu, and segregation of Cu elements will occur locally in the electrode material. On the one hand, the Mo element can improve this problem, so that the high entropy alloy produces an ordered strengthening phase, promotes the precipitation of the σ phase, suppresses the generation of defects, and further improves the hardness and strength of the electrode material. On the other hand, the atomic radius of Mo is significantly larger than the radius of other atoms. In this example, an excess of ammonium molybdate tetrahydrate is used, and the atoms undergo severe lattice distortion during the diffusion process. Compared with Example 2, the hardness of the electrode material is significantly reduced, and it is easy to break under high current impact.

[0114] Application Examples

[0115] The present invention also includes the study of hydrogen evolution electrode in the same project group, so the performance verification is carried out on the overall study. The oxygen evolution electrode prepared in Example 2 is used as the anode, and the hydrogen evolution electrode prepared by the following process is used as the counter electrode (cathode). A conventional water electrolysis system (pure water is used as the electrolyte raw material and a solid polymer membrane is used as the electrolytic membrane) is assembled. During the water electrolysis process, the constant current density is controlled to be 1.2A / cm 2 .

[0116] The hydrogen evolution electrode is prepared by the following process:

[0117] 1) Aluminum, copper and nickel were prepared in a mass ratio of 0.7:0.8:1, and aluminum, copper and nickel were repeatedly smelted three times at a temperature of 1460°C, and vacuum belted at a speed of 1500r / min, and rapidly cooled to obtain an alloy with a specification of 5cm×2cm×0.3cm, and the alloy was placed in a NaOH solution with a concentration of 5mol / L and ultrasonicated for 45min until there were no obvious bubbles to stop activation, and then washed and dried to obtain a conductive electrode;

[0118] 2) Take 0.27g of copper nitrate trihydrate, 1.82g of nickel nitrate, 0.5g of triethylamine, and 7mL of water and mix them evenly to obtain an aqueous solution. Put a conductive electrode into the aqueous solution and keep it at 120°C for 6 hours. Take out the conductive electrode and dry it.

[0119] 3) The conductive electrode was immersed in 15 mL of a 0.05 mol / L hydrogen sulfide solution at 110° C. for 7 h, and dried to obtain a hydrogen evolution electrode.

[0120] The cycle performance, oxygen evolution rate and hydrogen evolution rate of the water electrolysis system constructed in this example were characterized. The characterization results showed that after 72 hours of continuous operation, the decrease rate of hydrogen evolution performance and oxygen evolution performance were both ≤1‰, and the loss rate was ≤0.5‰, showing very excellent stability. At the same time, the hydrogen evolution rate and oxygen evolution rate reached about 85.1 mol·h -1 cm -1 and 42.6 mol·h -1 cm -1 When the two are used together, they show stronger hydrogen and oxygen evolution performance, which may be due to the synergistic effect brought about by the fact that neither of them will produce bubble adhesion and hinder the reaction.

[0121] Under the condition of high current density, a large number of bubbles will be generated on the electrode surface. When the bubbles gather and adhere to the vicinity of the active sites of the electrode material, an air cushion is formed, which causes the active sites to be "shielded," making it difficult for the electrolyte to diffuse, and the oxygen evolution rate is significantly reduced. Large bubbles have a greater ability to adhere to the electrode material, and may peel off the active substance. The present invention constructs a hydrophilic and air-repellent electrode surface by regulating the morphology of the surface of the active substance to avoid the formation of air cushions by bubbles, thereby causing the problem of "shielding" of the active sites. After characterization, it was found that the surface roughness of the oxygen evolution electrode prepared by the present invention is relatively large, and large bubbles can be divided into discontinuous small bubbles, that is, the generation of excessively large bubbles is avoided, the contact area between the bubbles and the electrode material is reduced, and the rapid desorption of bubbles is achieved. After observation, it can be seen that the oxygen evolution electrode and the hydrogen evolution electrode are surrounded by small bubbles, and they quickly rise to the surface of the electrolyte. After the bubbles are quickly desorbed, the active sites are exposed again, and the mass transfer of the electrolyte is promoted at the same time.

[0122] In summary, the oxygen evolution electrode prepared by the present invention has good application prospects.

Claims

1. A method for preparing a porous low-loss oxygen evolution electrode, characterized in that: The method comprises: 1) Take organic matter and mix it evenly, add excess calcium salt aqueous solution for suspension prepolymerization and polymerization, and obtain carbon-based materials through drying, preoxidation and heat treatment; 2) Mixing metal nitrate and organic solvent to obtain liquid phase A, mixing metal oxide acid salt and water to obtain liquid phase B, adding organic acid to the mixture of liquid phase A, liquid phase B and carbon-based material to react, and drying to obtain a composite material; 3) The composite material is subjected to heat treatment, and then rapidly cooled, cleaned and dried to obtain an oxygen evolution electrode.

2. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1, characterized in that: Step 1) The organic matter is divinylbenzene, styrene, or toluene; The divinylbenzene, styrene and toluene are prepared in a volume ratio of (1-1.2):1:(0.4-0.6).

3. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1, characterized in that: Step 1) The solute of the calcium salt aqueous solution is CaCl2, and its mass fraction is 1.2-1.8 wt%.

4. A method for preparing a porous low-loss oxygen evolution electrode according to claim 1, 2 or 3, characterized in that: Step 1) The suspension prepolymerization is carried out at a constant temperature of 50-60°C for 10-15 minutes; Step 1) The polymerization is carried out at 80-90°C for 7-8 hours; Step 1) The pre-oxidation is carried out in an air atmosphere at a constant temperature of 300-350°C for 4-5 hours; Step 1) The heat treatment is carried out under an inert atmosphere at a constant temperature of 600-650° C. for 1-2 h.

5. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1, characterized in that: Step 2) the metal nitrate is a mixture of nickel nitrate hexahydrate, iron nitrate nonahydrate, cobalt nitrate hexahydrate and copper nitrate trihydrate; The nickel nitrate hexahydrate, the iron nitrate nonahydrate, the cobalt nitrate hexahydrate, and the copper nitrate trihydrate are prepared in a mass ratio of (18-19.2): (6.7-8.3): (1.2-2.4): 1; Step 2) The organic solvent is ethanol, and the amount used is 8-10 mL / g metal nitrate.

6. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1, characterized in that: Step 2) the metal oxide acid salt is ammonium molybdate tetrahydrate, and its dosage is 1.5-2 g / g metal nitrate; In step 2), the amount of water used is 8-10 mL / g of metal oxide acid salt.

7. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1, characterized in that: Step 2) The amount of the carbon-based material is 1.5-2 g / mL of the total volume of the mixture of liquid phase A and liquid phase B; Step 2) The organic acid is citric acid, and the amount used is 0.3-0.4 g / g metal nitrate.

8. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1 or 7, characterized in that: Step 2) The reaction is carried out at 80-90°C in a water bath for 0.5-1 h.

9. The method for preparing a porous low-loss oxygen evolution electrode according to claim 1, characterized in that: Step 3) The heat treatment is carried out at 600-700°C for 4-5 hours.

10. A porous low-loss oxygen evolution electrode prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Hydrophilic carbon-based material modified high-entropy alloy water electrolysis hydrogen production catalyst as well as preparation method and application thereof

    CN119524874A