Nitrogen-doped hexagonal and cubic nickel ruthenium alloy electro-catalytic material as well as preparation method and application thereof
Nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic materials were prepared through hydrothermal method and plasma treatment, which solved the problems of traditional catalyst instability and low urea oxidation reaction efficiency in alkaline seawater electrolysis, and achieved efficient seawater hydrogen evolution and In the urea oxidation reaction, the overpotential of the catalyst is reduced and the cycle stability is improved.
Patent Information
- Application Number
- CN202311150247.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-07
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional catalysts are unstable in alkaline seawater electrolysis. The chlorine evolution reaction at the anode competes with the oxygen evolution reaction, resulting in low electrolysis efficiency and slow urea oxidation reaction kinetics, making it difficult to develop high-activity bifunctional catalysts.
Nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic materials were prepared using a hydrothermal method. A porous nanowire array structure was formed through plasma treatment, and then combined with high-temperature calcination to form a stable nitrogen-doped cubic phase to improve catalytic activity and stability.
The hydrogen evolution reaction in seawater and the urea oxidation reaction under high current density are efficiently carried out. The overpotential of the catalyst is reduced, the cycle stability is improved, and the catalytic activity is significantly enhanced. It is suitable for industrial standard current density.
Smart Images

Figure CN118727052A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new energy nanomaterial synthesis, and specifically relates to a nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material and a preparation method and application thereof. Background Art
[0002] Hydrogen (H2) is an energy carrier due to its 142MJ kg -1 The high energy density and zero emission of alkaline electrolyzers make them potential alternatives to traditional fossil fuels. The electrochemical hydrogen evolution reaction (HER) using renewable energy and alkaline electrolyzers can effectively reduce energy crises and environmental pollution. Considering the low availability of pure water, the use of seawater as a raw material for HER is a promising option. Therefore, the use of free and abundant seawater as a raw material for HER has attracted increasing attention. However, conventional catalysts are generally ineffective for alkaline seawater electrolysis due to their unstable nature. Another reason for the ineffectiveness of conventional catalysts is that the chlorine evolution reaction (CER) at the anode may compete with the oxygen evolution reaction (OER) for direct alkaline seawater electrolysis, because the thermodynamic potential of CER is only about 480 mV higher than that of OER, and the formation of corrosive hypochlorite may block and destroy the active sites of the catalyst, causing environmental hazards. Under alkaline conditions, CER can be prevented by limiting the overpotential (<0.48 V), however, the electrolysis of HER cannot reach the industrial standard (500-1000 mA cm -2 ).
[0003] Urea is an advanced hydrogen carrier with a hydrogen content of 6.67 wt%, and is a potential free source in human urine and urea-rich wastewater. Urea (CO(NH2)2) oxidation reaction (UOR) (CO(NH2)2+6OH - →N2(g)+5H2O(l)+CO2(g)+6e - , E0 = 0.37 V vs. RHE) is more efficient in producing hydrogen than OER (1.23 V vs. RHE). However, UOR is kinetically sluggish due to the complex six-electron transfer process and multiple formation / desorption of intermediates. Developing bifunctional cathode HER and anode UOR catalysts with high activity will reduce production costs, which remains a challenge.
[0004] NiRu alloy is one of the most effective catalysts for improving HER and UOR performance due to its low cost and inherent catalytic activity. So far, various strategies such as morphology and electronic structure modulation have been used to improve its catalytic performance. In addition, regulating the crystalline phase of NiRu alloy and adjusting the atomic arrangement and electronic structure is an effective means to regulate the catalytic activity of the catalyst. However, it is not easy to control the crystalline phase of NiRu alloy nanocatalysts under mild conditions. Summary of the invention
[0005] In view of the shortcomings of the prior art, the first object of the present invention is to provide a nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material, which has significant electrocatalytic performance and can solve the current problems of high current density seawater hydrogen evolution and urea oxidation reaction with high overpotential and low catalytic activity of the catalyst used.
[0006] The second object of the present invention is to provide a method for preparing the above electrocatalytic material, wherein the electrocatalytic material prepared by the method has a stable structure and a short synthesis time.
[0007] The third object of the present invention is to provide an application of the above-mentioned electrocatalytic material, which can be used for hydrogen evolution or urea oxidation in seawater under high current density and has good application prospects.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0009] A nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material, wherein the structure of the electrocatalytic material is a heterogeneous structure composed of a nitrogen-doped hexagonal nickel-ruthenium alloy and a face-centered cubic nickel-ruthenium alloy; the morphology of the electrocatalytic material is a porous nanowire array.
[0010] The preparation method of the electrocatalytic material comprises the following steps:
[0011] (1) A NiRu double hydroxide@Ni foam self-supporting electrode was prepared by a hydrothermal method;
[0012] (2) synthesizing the electrocatalytic material by using the nickel ruthenium double hydroxide@nickel foam self-supporting electrode prepared in step (1) through plasma treatment.
[0013] Furthermore, in step (1), the hydrothermal method for preparing the nickel-ruthenium double hydroxide @ nickel foam self-supporting electrode is specifically as follows: using nickel foam as a self-supporting carrier, dissolving nickel nitrate hexahydrate (Ni(NO3)2·6H2O), ruthenium trichloride hydrate (RuCl3·3H2O) and urea in deionized water, heating, and cooling to obtain the nickel-ruthenium double hydroxide @ nickel foam self-supporting electrode; the morphology of the nickel-ruthenium double hydroxide @ nickel foam self-supporting electrode is a nanowire array.
[0014] Furthermore, the heating conditions are a temperature of 120° C. and a time of 12 h; the molar volume ratio of the nickel nitrate hexahydrate, ruthenium trichloride hydrate, urea and deionized water is 0.01 mol: 0.24 mol: 0.5 mol: 3.5 L.
[0015] Furthermore, in step (2), the plasma treatment uses nitrogen or ammonia.
[0016] Furthermore, in step (2), the plasma treatment conditions are: power of 400-500 W, time of 5-15 min, and pressure of 30-60 Pa. Under these conditions, the nickel-ruthenium double hydroxide@nickel foam self-supporting electrode nanowire array can be converted into a nitrogen-doped hexagonal@cubic nickel-ruthenium alloy nanowire array.
[0017] Furthermore, washing and drying are required after cooling.
[0018] Furthermore, the washing is carried out using anhydrous ethanol; and the drying temperature is 60°C.
[0019] Furthermore, the electrocatalytic material prepared in step (2) can also be calcined to prepare nitrogen-doped cubic nickel-ruthenium alloy nanowire arrays, and the resulting product is recorded as N doped NiRu-fcc@NF. The calcination temperature is 300-700°C and the time is 1-6h.
[0020] An application of the above electrocatalytic material, wherein the electrocatalytic material can be used for hydrogen evolution from seawater or urea oxidation.
[0021] Beneficial effects:
[0022] (i) The nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material provided by the present invention has a stable structure and significant electrocatalytic performance, and can solve the current problems of high current density seawater hydrogen evolution and urea oxidation reaction with high overpotential and low catalytic activity of the catalyst.
[0023] (ii) The preparation method provided by the present invention is simple and fast, and the prepared electrocatalytic material has a stable structure and significant electrocatalytic performance. The present invention uses a hydrothermal method to prepare a self-supporting electrode NiRu-LDH@NF, treats the NiRu-LDH@NF self-supporting electrode with the help of plasma, and synthesizes a nitrogen-doped electrocatalytic material with a hexagonal@cubic nickel-ruthenium alloy nanowire array structure by in-situ nitridation of NiRu-LDH nanowires. At the same time, the present invention explores the influence of the crystal phase of the nickel-ruthenium alloy on the high current density hydrogen evolution and urea oxidation in seawater, providing a reference for the development of catalysts constructed by crystal surface engineering in the fields of hydrogen evolution and urea oxidation in seawater.
[0024] (III) The present invention uses room temperature plasma to treat NiRu-LDH@NF self-supporting electrodes to prepare nitrogen-doped hexagonal@cubic nickel-ruthenium alloy heterogeneous structure nanowire array electrocatalytic materials. The electrocatalytic materials synthesized by this method have stable structures and short synthesis time. High-energy species (free electrons, N, excited atoms, ionized atoms / molecules and free radicals) in the plasma system continuously attack the hydroxyl radicals of the NiRu-LDH@NF self-supporting electrode, and nitrogen doping leads to the reconstruction of its surface structure; mild and high-energy reaction conditions are used in room temperature plasma treatment to keep the arrangement of Ni and Ru atoms unchanged, thereby realizing the formation of nitrogen-doped hexagonal@cubic nickel-ruthenium alloy heterogeneous structure nanowire arrays. Therefore, the NiRu-LDH@NF self-supporting electrode is in-situ nitrided by nitrogen or ammonia plasma, and a stable nitrogen-doped hexagonal@cubic nickel-ruthenium alloy heterogeneous structure nanowire array electrocatalytic material can be synthesized, and the synthesis time used is short. In addition, nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalyst material can be converted into thermodynamically stable nitrogen-doped cubic phase nickel-ruthenium alloy nanowire array electrocatalyst material through high-temperature calcination in an inert atmosphere.
[0025] (IV) The nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalyst provided by the present invention has high activity and good stability. It is applied to the hydrogen evolution reaction of seawater and the urea oxidation reaction at a high current density and exhibits significant catalytic activity. Compared with the nitrogen-doped cubic nickel-ruthenium alloy electrocatalyst (N doped NiRu-fcc@NF), the prepared nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalyst (N doped NiRu-inf@NF) catalyst exhibits significantly enhanced activity. When N dopedNiRu-inf@NF is applied to the hydrogen evolution reaction (HER) of seawater, the catalytic activity is significantly enhanced at 1000mAcm -2 At a current density of 1.5 V, the overpotential is 231 mV, and the cycle stability is as long as 100 h. When N doped NiRu-inf@NF is applied to urea oxidation reaction (UOR), only 1.34 V vs. RHE is required to achieve 100 mA cm -2 In addition, the alkaline electrolyzer assembled with N doped NiRu-inf@NF as anode and cathode only needs 1.36V voltage to reach 100mAcm when urea is decomposed in 1M KOH. -2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic diagram of the application of N doped NiRu-inf@NF prepared in Example 1;
[0027] Figure 2are XRD spectra of NiRu-LDH@NF, N doped NiRu-inf@NF, N doped NiRu-inf-1@NF prepared in Example 1 and N doped NiRu-fcc@NF prepared in Example 2;
[0028] Figure 3 The SEM images of NiRu-LDH@NF and N doped NiRu-inf@NF prepared in Example 1 and N doped NiRu-fcc@NF prepared in Example 2 are shown; Figure 3 (a) is a high-magnification SEM image of NiRu-LDH@NF. Figure 3 (b) is a low-magnification SEM image of NiRu-LDH@NF. Figure 3 (c) is a high magnification SEM image of N doped NiRu-inf@NF. Figure 3 (d) is a low-magnification SEM image of N doped NiRu-inf@NF. Figure 3 (e) is a high-magnification SEM image of N doped NiRu-fcc@NF. Figure 3 (f) is a low-magnification SEM image of N doped NiRu-fcc@NF;
[0029] Figure 4 Schematic diagram of contact angles of pure nickel foam and N doped NiRu-inf@NF prepared in Example 1; Figure 4 (a) is a schematic diagram of the contact angle of pure nickel foam. Figure 4 (b) is a schematic diagram of the contact angle of N doped NiRu-inf@NF prepared in Example 1;
[0030] Figure 5 LSV curves of HER of NiRu-LDH@NF, N doped NiRu-inf@NF prepared in Example 1, N doped NiRu-fcc@NF prepared in Example 2, N doped NF prepared in Comparative Example 1, and NiRu-C@NF prepared in Comparative Example 2;
[0031] Figure 6 is the LSV curve of HER of N doped NiRu-inf@NF prepared in Example 1 at different temperatures;
[0032] Figure 7The LSV curves of UOR of NiRu-LDH@NF, N doped NiRu-inf@NF prepared in Example 1, N doped NiRu-fcc@NF prepared in Example 2, N doped NF prepared in Comparative Example 1, and NiRu-C@NF prepared in Comparative Example 2 are shown;
[0033] Figure 8 This is the LSV curve of the alkaline electrolyzer assembled with the N doped NiRu-inf@NF prepared in Example 1 as the anode and cathode for seawater splitting and urea splitting under 1 M KOH conditions. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but this is not intended to limit the present invention.
[0035] Unless otherwise specified, the content of each component used below is in mass percentage.
[0036] Embodiment 1
[0037] (1) Weighing 0.0414 g (0.0002 mol) of RuCl3·3H2O, 1.3956 g (0.0048 mol) of Ni(NO3)2·6H2O, and 0.6004 g (0.01 mol) of urea, respectively, and dissolving them in 70 mL of deionized water to obtain a mixed solution; transferring the mixed solution to a 100 mL polytetrafluoroethylene-lined autoclave, and immersing the cleaned nickel foam in the mixed solution, heating it in an oven set at 120°C for 12 hours, and after cooling, taking out the nickel foam immersed in the mixed solution, washing the surface impurity ions with anhydrous ethanol, and then drying it in an oven at 60°C to prepare a NiRu-LDH@NF self-supporting electrode;
[0038] (2) treating the NiRu-LDH@NF self-supporting electrode prepared in step (1) with nitrogen plasma at a power of 400 W, a time of 15 min, and a pressure of 60 Pa to obtain a nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material, denoted as N doped NiRu-inf@NF;
[0039] (3) The NiRu-LDH@NF self-supporting electrode prepared in step (1) was treated with nitrogen plasma at a power of 500 W, a time of 5 min, and a pressure of 30 Pa. A nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material was also prepared, which was denoted as N doped NiRu-inf-1@NF.
[0040] Embodiment 2
[0041] (1) Same as step (1) of Example 1;
[0042] (2) Same as step (2) of Example 1;
[0043] (3) The N doped NiRu-inf@NF prepared in step (2) is placed in the tube cavity of a tubular furnace and calcined at a high temperature of 500°C for 3 hours in a nitrogen atmosphere to obtain a nitrogen-doped cubic nickel-ruthenium alloy electrocatalyst material, which is recorded as N doped NiRu-fcc@NF.
[0044] Figure 2 The XRD spectra of NiRu-LDH@NF prepared in step (1) of Example 1, N doped NiRu-inf@NF prepared in step (2), N doped NiRu-inf-1@NF prepared in step (3) and N doped NiRu-fcc@NF prepared in Example 2 are shown respectively. Firstly, in order to eliminate the interference of the foam nickel base peak on our samples, we ultrasonically tested the phase of the powder sample when testing XRD. First, the NiRu-LDH@NF self-supporting electrode was successfully synthesized by a simple hydrothermal method. When treated in a nitrogen plasma atmosphere for 15 minutes, diffraction peaks appeared at 39.1°, 41.5°, 44.5°, 58.4°, and 70.98°, corresponding to the (010), (002), (011), (012), and (110) crystal planes, respectively, indicating that the metastable hexagonal phase (hcp) of the NiRu alloy was successfully synthesized. In addition, a (200) diffraction peak appeared at 51.8°, corresponding to face-centered cubic (fcc) Ni, which means that after plasma nitridation treatment, a NiRu heterogeneous structure composed of hcp and fcc was successfully constructed. After high-temperature calcination of N doped NiRu-inf@NF, the XRD curve of N doped NiRu-fcc@NF showed that the hcp had been completely transformed into a stable fcc phase. In addition, no diffraction peak of nickel nitride appears in the XRD curve. We speculate that only a small amount of nitrogen is doped in the NiRu alloy during plasma nitridation, and no new phase is formed. In summary, appropriate plasma treatment time is crucial to the formation of heterogeneous structure of N-doped NiRu alloy.
[0045] Figure 3 (a) and Figure 3 (b) are low-magnification SEM and high-magnification SEM images of the NiRu-LDH@NF self-supporting electrode prepared in step (1) of Example 1, respectively. The results show that the NiRu-LDH@NF nanowire array grows vertically on the nickel foam, the surface of the nanowire is relatively smooth, the diameter of the nanowire is about 50-100 nm, and the length is about 300-400 nm. Under a low-magnification electron microscope, it is shown that the nanowire grows uniformly on the nickel foam; Figure 3 (c) and Figure 3 (d) are low-magnification SEM and high-magnification SEM images of the N doped NiRu-inf@NF prepared in Example 1. After the NiRu-LDH@NF self-supporting electrode was treated with nitrogen plasma for 15 min, the surface structure of the nanowires became rough and numerous nanopores were formed. The abundant pores can expose abundant active sites, which is convenient for the contact area between the nanocatalyst and the electrolyte, and is beneficial to accelerate charge transfer and mass diffusion, thereby greatly improving the electrocatalytic hydrogen evolution performance. Figure 3 (e) and Figure 3 (f) is the low-magnification SEM and high-magnification SEM images of the N doped NiRu-fcc@NF prepared in Example 2. After high-temperature calcination, the nanowire array collapses severely and it is difficult to find the nanowires microscopically.
[0046] The wettability of the electrode is also an important factor in driving the HER process at high current density, because the continuous and violent bubbles generated during the HER process at high current density adhere to the catalyst surface, which will hinder the charge and mass transfer at the solid-liquid interface, block the active sites, and are not conducive to the enhancement of HER activity. Figure 4 The contact angle of N dopedNiRu-inf@NF and pure nickel foam prepared in Example 1 was characterized by a contact angle instrument. The contact angle of N doped NiRu-inf@NF was 0°, which was significantly smaller than that of NF. The results show that compared with the hydrophobic NF electrode, N doped NiRu-inf@NF exhibits obvious superhydrophilicity, which is conducive to the wetting of the electrolyte, and the hydrogen bubbles under the electrolyte escape from the electrode surface and provide sufficient active sites, thereby promoting the HER, especially at high current density.
[0047] Comparative Example 1
[0048] Preparation of N doped NF self-supporting electrodes:
[0049] Pure nickel foam was treated with nitrogen plasma at a power of 400 W, a time of 15 min, and a pressure of 60 Pa to prepare nitrogen-doped nickel foam, which was recorded as N doped NF.
[0050] Comparative Example 2
[0051] Preparation of NiRu-C@NF self-supporting electrode:
[0052] (1) Same as step (1) of Example 1;
[0053] (2) The NiRu-LDH@NF self-supporting electrode prepared in step (1) was calcined in argon at a temperature of 500° C. for 3 h to synthesize a nickel-ruthenium alloy@nickel foam electrocatalyst material, which was recorded as NiRu-C@NF.
[0054] Performance Testing
[0055] The HER and UOR performances of the electrocatalytic materials prepared in Examples 1 and 2 were tested at high current density. Figure 5 The NiRu-LDH@NF, N doped NiRu-inf@NF prepared in Example 1, N doped NiRu-fcc@NF and pure NF prepared in Example 2, N doped NF prepared in Comparative Example 1, and NiRu-C@NF prepared in Comparative Example 2 were tested at 5 mV·s -1 The LSV curves of HER were obtained at a scan rate of 100 mA cm-1. The results show that the activity of NF and N doped NF for HER is negligible. After plasma treatment, the alkaline hydrogen evolution performance of the prepared N doped NiRu-inf@NF is significantly improved. NiRu-LDH@NF, N doped NiRu-inf@NF, N doped NiRu-fcc@NF and NiRu-C@NF are -2 The overpotentials at different current densities are 237.6mV, 81.6mV, 172mV, and 134.7mV respectively. Among them, the N doped NiRu-inf@NF sample has the lowest overpotential of 81.6mV. At high current density, the current density of N doped Ru-inf@NF can reach 1400mAcm -2 , at 1000mAcm -2 The N doped NiRu-inf@NF prepared in Example 1 of the present invention has an overpotential of 231 mV at a current density of .
[0056] The HER performance of the N doped NiRu-inf@NF prepared in Example 1 was tested at different temperatures of 20°C, 40°C, 60°C, and 80°C. Figure 6 It can be seen that when the electrolyte temperature increases, the catalytic activity of N doped NiRu-inf@NF as an electrode material also increases. -2 At a current density of 1.3 Å, N doped NiRu-inf@NF has an overpotential of 142 mV.
[0057] Depend on Figure 7It can be seen that under the UOR condition, N doped NF, NiRu-LDH@NF, N doped NiRu-inf@NF, N doped NiRu-fcc@NF and NiRu-C@NF have the highest conductivity at 100 mA cm -2 The potentials at the current densities are 1.43 V, 1.37 V, 1.34 V, 1.36 V, and 1.40 V, respectively. The potential of N doped NiRu-inf@NF is the lowest, indicating that it has strong urea oxidation performance.
[0058] The LSV curves of the alkaline electrolyzer assembled with N doped NiRu-inf@NF prepared in Example 1 as anode and cathode (N doped NiRu-inf@NF||N doped NiRu-inf@NF) for seawater splitting and urea splitting in 1M KOH are as follows: Figure 8 As shown in Figure 2, N doped NiRu-inf@NF only needs 1.36 V to achieve 100 mA cm for urea decomposition. -2 , N doped NiRu-inf@NF requires 1.607V voltage to achieve 100mAcm when performing seawater splitting -2 .
[0059] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A nitrogen-doped hexagonal@cubic nickel-ruthenium alloy electrocatalytic material, It is characterized in that The structure of the electrocatalytic material is a heterogeneous structure composed of nitrogen-doped hexagonal nickel-ruthenium alloy and face-centered cubic nickel-ruthenium alloy; the morphology of the electrocatalytic material is a porous nanowire array.
2. A method for preparing the electrocatalytic material according to claim 1, It is characterized in that The preparation method adopts the following steps: (1) Preparation of NiRu double hydroxide@Ni foam self-supporting electrode by hydrothermal method; (2) Synthesizing the electrocatalytic material by using the nickel-ruthenium double hydroxide@nickel foam self-supporting electrode prepared in step (1) through plasma treatment.
3. The preparation method according to claim 2, It is characterized in that In step (1), the hydrothermal method for preparing the nickel-ruthenium double hydroxide @ nickel foam self-supporting electrode is specifically as follows: using nickel foam as a self-supporting carrier, dissolving a certain proportion of nickel nitrate hexahydrate, ruthenium trichloride hydrate and urea in deionized water, heating, and cooling to obtain the nickel-ruthenium double hydroxide @ nickel foam self-supporting electrode.
4. The preparation method according to claim 3, It is characterized in that The heating conditions are as follows: temperature 120° C., time 12 h; the molar volume ratio of the nickel nitrate hexahydrate, ruthenium trichloride hydrate, urea and deionized water is 0.01 mol: 0.24 mol: 0.5 mol: 3.5 L.
5. The preparation method according to claim 2, It is characterized in that In step (1), the morphology of the nickel-ruthenium double hydroxide@nickel foam self-supporting electrode is a nanowire array.
6. The preparation method according to claim 2, It is characterized in that In step (2), the plasma treatment uses nitrogen or ammonia; the conditions of the plasma treatment are power 400-500 W, time 5-15 min, and pressure 30-60 Pa.
7. The preparation method according to claim 3, It is characterized in that After the cooling, washing and drying are required.
8. The preparation method according to claim 7, It is characterized in that The washing method uses anhydrous ethanol; the drying temperature is 60°C.
9. The preparation method according to claim 2, It is characterized in that The electrocatalytic material prepared in step (2) can also be calcined to prepare nitrogen-doped cubic nickel-ruthenium alloy nanowire arrays, wherein the calcination temperature is 300-700° C. and the calcination time is 1-6 h.