Cystamine-based lead-free perovskite single crystal and preparation method and application thereof
By introducing cysteamine as an organic spacer cation into tin-based perovskite, and using the diamine layer connected by S-S bonds, high-quality cysteamine tin-based perovskite single crystals and films were prepared, solving the problem of tin-based perovskite Solve the stability and performance issues of optoelectronic devices, achieve higher stability and conductivity, and significantly improve optoelectronic performance.
Patent Information
- Application Number
- CN202410584607.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-12
- Publication Date
- 2024-10-01
AI Technical Summary
Existing tin-based perovskite optoelectronic devices have low photoelectric performance and poor stability. The main reason is that divalent tin ions are easily oxidized to tetravalent tin ions, and the active phase transition of the three-dimensional structure results in short service life.
Using cysteamine as a non-lead organic spacer cation, the diamine layer connected by S-S bond is inserted into the tin-based inorganic layer to prepare rhombic sheet-shaped (2-AET)2An-1SnnX3n+1 type cysteamine tin-based calcium Titanium single crystal, and high-quality single crystals and films are obtained through specific synthesis methods to enhance the stability and conductivity of the material.
The stability and photoelectric performance of tin-based perovskite are improved. The surface of the single crystal is dense and smooth, and it still maintains its original shape when exposed to the air. The conductivity of the two-dimensional perovskite is enhanced, and high-quality films are prepared by back-melting to reduce the photovoltaic performance. The grain boundary defect density of the device significantly improves device performance.
Smart Images

Figure CN118727121A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of perovskite photoelectric devices, and specifically relates to a cysteamine-based non-lead perovskite single crystal and a preparation method and application thereof. Background Art
[0002] In recent years, perovskite materials have attracted extensive attention from the scientific research and industry circles due to their excellent optoelectronic properties such as high carrier mobility, high absorption coefficient and high fluorescence quantum yield. They have broad application prospects and large development space. Traditional perovskite optoelectronic devices inevitably contain lead elements, which cause lead toxicity and hinder their industrial application. The chemical properties of tin are similar to those of lead, but the toxicity is lower, and the band gap of tin-based perovskite materials is narrower and more stable than that of lead-based perovskite materials. Therefore, in-depth research on tin-based perovskites is an effective way to avoid lead poisoning.
[0003] However, the main reason why the photoelectric performance of existing tin-based perovskite devices is not high is that divalent tin ions (Sn 2+ ) is easily affected by environmental factors and oxidized to tetravalent tin ions (Sn 4+ ), losing the original photoelectric performance. In addition, the three-dimensional structure of perovskite materials will also cause active phase transitions due to factors such as ion migration and volatilization, which seriously weakens the service life of perovskite photoelectric devices. Compared with traditional three-dimensional perovskites, two-dimensional perovskite materials have large formation energy and high structural stability. Therefore, exploring new organic spacer cations and regulating the crystallization of two-dimensional tin-based perovskites can fundamentally improve the stability of perovskite photoelectric devices.
[0004] There are many reports on the application of cysteamine in perovskite optoelectronic devices. For example, Prachi Kour et al. prepared (2-AET)7Pb4I 15 Perovskite-like single crystals were used to study the phase transition process between (2-AET)2PbI4 and the existence form of cysteamine ions in acidic and alkaline media, and a (2-AET)7Pb4I 15self-powered photodetector (Angew.Chem.Int.Ed.2021,60,18750-18760); Zhexin Song et al. synthesized (2-AET)2SnI4 single crystals by slow volatilization method, and exposed them to H3PO2 solution and ambient atmosphere, showing a reversible red-black transition (Inorg.Chem.2022,61,6943-6952); Chenghao Bi et al. used cysteamine instead of the original long-chain ligands such as oleic acid (OA) and oleylamine (OAm) to synthesize CsPbI3 perovskite quantum dots (ODs), and finally prepared a photodetector based on AET-CsPbI3QD film. The AET-CsPbI3 QD photodetector still maintains an initial response rate of more than 95% after being immersed in water for 1 hour or irradiated with ultraviolet light for 2 hours without external bias and any packaging. (Adv. Funct. Mater. 2019, 29, 1902446). In addition, because the strong interaction between Pb-S can change the work function of the perovskite material, cysteamine can be used as a perovskite work function regulator to prepare perovskite solar cells with high open circuit voltage (see invention patent No. CN115768228A).
[0005] Although cysteamine has been widely used in perovskite optoelectronic devices, there has been no report on using cysteamine ions as organic spacer cations of non-lead two-dimensional perovskites to prepare perovskite single crystals with different n values and optoelectronic devices based on perovskite films with different n values. Summary of the invention
[0006] The present invention provides a cysteamine-based non-lead perovskite single crystal and a preparation method and application thereof, which further improves the photoelectric performance of existing two-dimensional tin-based perovskite devices while avoiding lead poisoning and improving stability.
[0007] The cysteamine-based non-lead perovskite single crystal of the present invention has a general structural formula of (2-AET)2A n-1 Sn n X 3n+1 In the single crystal structure, cysteamine is used as a spacer cation, and a diamine organic layer connected by SS bonds is inserted between two tin-based inorganic layers.
[0008] Among them, A in the general structural formula is methylamine ion (FA + ), formamidinium ion (MA + ) in one or more; X is Cl - Br - ,I - One or more of; wherein 1≤n≤6 is an integer.
[0009] Wherein, the single crystal is a diamond-shaped flake centimeter-level single crystal; when n=1, the single crystal is red; when n=2, the single crystal is dark red; when 3≤n≤6, the single crystal is black.
[0010] The method for preparing the above-mentioned cysteamine tin-based perovskite single crystal comprises the following steps:
[0011] (1) dissolving SnI2 in HI solution to obtain a mixed solution of SnI2 and HI;
[0012] (2) dissolving a cysteamine halide and an organic halide in a HI solution to obtain a mixed solution of a cysteamine halide [(2-AET)X], an organic halide and HI;
[0013] (3) adding a mixed solution of (2-AET)X, an organic halide and HI to a mixed solution of SnI2 and HI to obtain a mixed solution of (2-AET)X, an organic halide, SnI2 and HI;
[0014] (4) adding H3PO2 solution to the mixed solution of (2-AET)X, organic halide, SnI2 and HI to obtain a mixed solution of H3PO2, (2-AET)X, organic halide, SnI2 and HI;
[0015] (5) The mixed solution of H3PO2, (2-AET)X, organic halide, SnI2 and HI is heated until the solution is clear and then cooled to room temperature to obtain (2-AET)2A n-1 Sn n X 3n+1 A mixture of crystals and mixed solution.
[0016] (6) The above (2-AET)2A n-1 Sn n X 3n+1 The mixture of the crystals and the mixed solution was filtered under reduced pressure, and ether was slowly added dropwise to wash until the filtrate was colorless to obtain wet (2-AET)2A. n-1 Sn n X 3n+1 Crystal.
[0017] (7) The above wet (2-AET)2A n-1 Sn n X 3n+1 The crystals are placed in a vacuum oven and dried to obtain pure (2-AET)2A. n-1 Sn n X 3n+1 Crystal.
[0018] Wherein, in step (1), the HI solution is prepared by mixing HI and deionized water, with a mass fraction of 47-57%; the molar ratio of HI to SnI2 is 12-16:1; and the dissolution temperature is 70-90°C.
[0019] Wherein, in step (2), the molar ratio of HI to cysteamine is 3.5-4.5:1; the molar ratio of HI to cysteamine halide is 2.5-3.5:1; and the dissolution temperature is room temperature.
[0020] Wherein, in step (2), the organic halide comprises one or more of methylamine halide and formamidine halide
[0021] Wherein, in step (2), when n=1, the solution does not contain organic halide; when n=2, the molar ratio of cysteamine halide to organic halide is 2:1; when n=3, the molar ratio of cysteamine halide to organic halide is 1:1; when n=4, the molar ratio of cysteamine halide to organic halide is 2:3; when n=5, the molar ratio of cysteamine halide to organic halide is 1:2; when n=6, the molar ratio of cysteamine halide to organic halide is 2:5.
[0022] Wherein, in step (3), the mixed solution of (2-AET)X, organic halide and HI is added to the mixed solution of SnI2 and HI at a rate of 1 to 1.5 mL / min.
[0023] Wherein, in step (4), the H3PO2 solution is prepared by mixing H3PO2 and deionized water, with a mass fraction of 50%; the molar ratio of HI to H3PO2 is 8 to 10:1.
[0024] Wherein, in step (5), the heating temperature is 90-120°C; the cooling rate is 3-3.5°C / h, and the crystallization time is 20-23h. The nucleation rate can be slowed down by slowly cooling down, resulting in fewer nuclei, thereby obtaining larger crystals with full and regular grains.
[0025] Wherein, in step (6), the rate of slow dripping is 2 to 3 mL / min.
[0026] Wherein, in step (7), the drying temperature is 35 to 45° C. and the drying time is 25 to 35 minutes.
[0027] All the above steps were carried out in a nitrogen atmosphere with an oxygen content below 0.01 ppm.
[0028] The present invention also provides a perovskite solar cell prepared from the cysteamine-based non-lead perovskite single crystal.
[0029] The present invention also provides a perovskite photodetector prepared from the cysteamine-based non-lead perovskite single crystal.
[0030] Compared with the prior art, the present invention has the following advantages:
[0031] (1) The present invention uses a two-step method to mix cysteamine or its halide, organic halide and SnI2 in HI solution, and then slowly cools down to synthesize rhombic flake centimeter-scale single crystal (2-AET)2A n-1 Sn n X 3n+1 The single crystal surface is dense and flat, the overall size is large, and a clear geometric configuration is formed.
[0032] (2) The cysteamine cations in the single crystal are connected by SS bonds, which have a stronger interaction strength than the van der Waals force, forming a unique diamine layer, which greatly improves the stability of the tin-based perovskite and maintains the original crystal form after being exposed to air for 1 hour. The presence of p-orbital electrons in the SS bonds enhances the conductivity of the two-dimensional perovskite.
[0033] (3) The single crystal preparation process of the present invention is simple and reproducible, and the preparation time is greatly shortened on the basis of forming high-quality single crystals.
[0034] (4) The single crystal can be dissolved back to prepare high-quality, stoichiometric tin-based two-dimensional perovskite films based on seed memory; the defect density at the grain boundaries of the perovskite layer of the optoelectronic device can be reduced, greatly improving the performance of the optoelectronic device. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 =(2-AET)2A n-1 Sn n X 3n+1 Schematic diagram of the crystal structure
[0036] Figure 2 Macroscopic photo of (2-AET)2SnI4 single crystal of Example 1
[0037] Figure 3 Scanning electron microscope photo of (2-AET)2SnI4 single crystal of Example 1
[0038] Figure 4 Schematic diagram of the structure of the photodetector made of (2-AET)2SnI4 single crystal in Example 1
[0039] Figure 5 (2-AET)2FA3Sn4I of Example 2 13 Schematic diagram of the structure of a solar cell made of a single crystal
[0040] in, Figure 4111 and 112 are gold electrodes, 120 is a (2-AET)2SnI4 perovskite layer, and 130 is a quartz substrate; Figure 5 210 is a silver electrode, 220 is a BCP hole blocking layer, 230 is a PCBM electron transport layer; 240 is (2-AET)2FA3Sn4I 13 Perovskite layer; 250 is PEDOT:PSS hole transport layer; 260 is FTO conductive glass. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] (1) Preparation of (2-AET) 2SnI4 single crystals. The entire preparation process was carried out in a nitrogen atmosphere with an oxygen content below 0.01 ppm:
[0044] Weigh 372.52 mg of stannous iodide (SnI2) into a clean reagent bottle, use a pipette to transfer 1.5 mL of 57% hydroiodic acid (HI) solution, add a clean stirring bar, and cover the bottle cap; heat and stir at 90°C and a stirring rate of 3000 r / min for 20 min until the solution is completely clarified to obtain a mixed solution of SnI2 and HI.
[0045] Weigh 77.14 mg of cysteamine into a clean reagent bottle, use a pipette to transfer 0.45 mL of 57% hydroiodic acid (HI) solution, and cover the bottle cap; shake the reagent bottle at room temperature until the solution is completely clear to obtain a mixed solution of (2-AET)I and HI.
[0046] The mixed solution of (2-AET)I and HI was added dropwise to the mixed solution of SnI2 and HI at a rate of 1.5 mL / min to obtain a mixed solution of (2-AET)I, SnI2 and HI; and 0.25 mL of 50% hypophosphorous acid (H3PO2) solution was added thereto to obtain a mixed solution of H3PO2, (2-AET)I, SnI2 and HI.
[0047] The mixed solution of H3PO2, (2-AET)I, SnI2 and HI was heated and stirred at 110°C and 3000 r / min for 40 min until the solution was completely clear; and placed on a hot plate at 110°C, and the program was set to cool from 110°C to 25°C for 24 h. After 24 h, a mixture of (2-AET)2SnI4 crystals and the mixed solution was obtained.
[0048] The mixture was filtered under reduced pressure, and ether was slowly added dropwise for washing. After the amount of ether added was increased to 100 mL, the filtrate was colorless, and wet (2-AET)2SnI4 single crystals were obtained. The wet crystals were placed in a constant temperature drying oven at 40°C and dried for 30 min to obtain 450.23 mg of pure (2-AET)2SnI4 single crystals with a yield of 64%.
[0049] (2) Preparation of photodetector based on (2-AET)2SnI4 single crystal:
[0050] Add 0.64 mL of γ-butyrolactone (GBL) solution to the above pure (2-AET)2SnI4 single crystal; shake and stir the bottle until the crystal is completely dissolved in the GBL solution, stir for 24 hours in a nitrogen atmosphere to prepare a clear 1 mol / L (2-AET)2SnI4 precursor solution.
[0051] The quartz sheets (10 mm*10 mm) were continuously ultrasonically washed in deionized water, acetone, ethanol and isopropanol for 15 min, then dried by nitrogen blowing and treated with UV / ozone for 25 min; two UV / ozone treated quartz sheets were placed on a hot plate at 105°C for preheating with the hydrophobic side facing up, and the (2-AET)2SnI4 precursor solution was placed on the hot plate for preheating.
[0052] Use a pipette to transfer 5 μL of the precursor solution onto the hydrophobic surface of the quartz plate, and then press the hydrophobic surface of another quartz plate onto the substrate. Keep the temperature of the hot plate at 105°C for 1.5 hours, then increase the temperature by 1°C every 12 minutes until the temperature reaches 125°C. Keep the temperature of the hot plate at 125°C for 20 hours, and then grow a (2-AET)2SnI4 single crystal thin film;
[0053] A metal template with a channel width of 30 μm is covered on the surface of the single crystal thin slice; it is placed in a vacuum evaporator, and after slowly and evenly evaporating a 70 nm gold electrode, the metal template is removed to obtain a photodetector based on the (2-AET)2SnI4 single crystal.
[0054] Example 2
[0055] (1)(2-AET)2FA3Sn4I 13The preparation of single crystals is carried out in a nitrogen atmosphere with an oxygen content below 0.01ppm:
[0056] Weigh 372.52 mg of stannous iodide (SnI2) into a clean reagent bottle, use a pipette to transfer 1.5 mL of 57% hydroiodic acid (HI) solution, add a clean stirring bar, and cover the bottle cap; heat and stir at 90°C and a stirring rate of 3000 r / min for 20 min until the solution is completely clarified to obtain a mixed solution of SnI2 and HI.
[0057] Weigh 38.57 mg of cysteamine and 128.98 mg of formamidine iodide (FAI) into a clean reagent bottle, use a pipette to transfer 0.45 mL of 57% hydroiodic acid (HI) solution, and cover the bottle cap; shake the reagent bottle at room temperature until the solution is completely clear to obtain a mixed solution of (2-AET)I, FAI and HI.
[0058] The mixed solution of (2-AET)I, FAI and HI was added dropwise to the mixed solution of SnI2 and HI at a rate of 1.5 mL / min to obtain a mixed solution of (2-AET)I, FAI, SnI2 and HI; and 0.25 mL of 50% hypophosphorous acid (H3PO2) solution was added thereto to obtain a mixed solution of H3PO2, (2-AET)I, FAI, SnI2 and HI.
[0059] The mixed solution of H3PO2, (2-AET)I, FAI, SnI2 and HI was heated and stirred at 110°C and 3000 r / min for 40 min until the solution was completely clear; and then placed on a hot plate at 110°C and programmed to cool from 110°C to 25°C for 24 h. After 24 h, (2-AET)2FA3Sn4I 13 A mixture of crystals and mixed solution.
[0060] The mixture was filtered under reduced pressure, and ether was slowly added dropwise to wash. After 130 mL of ether was added dropwise, the filtrate was colorless to obtain wet (2-AET)2FA3Sn4I 13 Single crystal; Place the wet crystal in a 40°C constant temperature drying oven and dry for 30 minutes to obtain pure (2-AET)2FA3Sn4I 13 Single crystal 193.42 mg, yield 29%.
[0061] (2) Preparation of solar cells based on (2-AET)2SnI4 single crystals:
[0062] NH4SCN and NH4Cl were used as vertical induction agents, and DMF and DMSO were used as solvents. The solute ratio was: (2-AET)2FA3Sn4I 13:NH4SCN:NH4Cl=5:5:1 (molar ratio), the solvent ratio is DMSO:DMF=4:1, take the above pure (2-AET)2FA3Sn4I 13 193.42 mg of single crystal was obtained. The solute and solvent were mixed and the solution was stirred for more than 5 hours until it became clear, and 0.3 mL of perovskite precursor solution was obtained.
[0063] The FTO conductive glass (10mm*10mm) was continuously ultrasonically washed in deionized water, acetone, ethanol and isopropanol for 15 minutes, then dried by blowing with nitrogen and treated with UV / ozone for 25 minutes; after filtering with a 0.22μm filter head, PEDOT:PSS was spin-coated on the FTO substrate, baked on a hot stage at 150°C for 10 minutes and then taken out to obtain a hole transport layer with a thickness of 50nm.
[0064] The prepared precursor solution (50 μL) was dropped onto the hole transport layer and spin-coated at 3000 rpm for 30 s. Finally, it was annealed on a hot plate at 100 °C for 5 min and cooled to room temperature to obtain (2-AET)2FA3Sn4I 13 Perovskite layer.
[0065] In (2-AET)2FA3Sn4I 13 The PCBM electron transport layer and BCP hole blocking layer were spin-coated on the perovskite layer, with the spin-coating time of 30s and 40s, and the spin-coating speed of 3000r / min and 4000r / min, respectively, and finally the Ag electrode was evaporated. The final structure was FTO / PEDOT:PSS / (2-AET)2FA3Sn4I 13 High-efficiency and high-stability two-dimensional tin-based perovskite solar cells with two-dimensional tin-based perovskite layer / PCBM / BCP / Ag.
Claims
1. A method for preparing a cysteamine tin-based perovskite single crystal, characterized in that: The steps include: Dissolving SnI2 in HI solution to obtain a mixed solution of SnI2 and HI; Dissolve cysteamine halide and organic halide in HI solution to obtain a mixed solution of cysteamine halide [(2-AET)X], organic halide and HI; add the mixed solution of (2-AET)X, organic halide and HI to the mixed solution of SnI2 and HI to obtain a mixed solution of (2-AET)X, organic halide, SnI2 and HI; add H3PO2 solution to the mixed solution of (2-AET)X, organic halide, SnI2 and HI to obtain a mixed solution of H3PO2, (2-AET)X, organic halide, SnI2 and HI; heat the mixed solution of H3PO2, (2-AET)X, organic halide, SnI2 and HI until the solution is clear and then cool to room temperature to obtain (2-AET)2A n-1 Sn n X 3n+1 A mixture of crystals and mixed solution. The above (2-AET)2A n-1 Sn n X 3n+1 The mixture of crystals and mixed solution was filtered under reduced pressure, and ether was slowly added dropwise to wash until the filtrate was colorless to obtain wet (2-AET)2A. n-1 Sn n X 3n+1 Crystals. The above wet (2-AET)2A n- 1Sn n X 3n+1 The crystals are placed in a vacuum oven and dried to obtain pure (2-AET)2A. n-1 Sn n X 3n+1 Crystal.
2. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, wherein: The HI solution is prepared by mixing HI and deionized water, with a mass fraction of 47-57%; the molar ratio of HI to SnI2 is 12-16:1; and the dissolution temperature is 70-90°C.
3. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The molar ratio of HI to cysteamine is 3.5-4.5:1; the molar ratio of HI to cysteamine halide is 2.5-3.5:1; and the dissolution temperature is room temperature.
4. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The organic halide includes one or more of methylamine halide and formamidine halide.
5. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: When n=1, the solution does not contain organic halide; when n=2, the molar ratio of cysteamine halide to organic halide is 2:1; when n=3, the molar ratio of cysteamine halide to organic halide is 1:1; when n=4, the molar ratio of cysteamine halide to organic halide is 2:3; when n=5, the molar ratio of cysteamine halide to organic halide is 1:2; when n=6, the molar ratio of cysteamine halide to organic halide is 2:
5.
6. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The rate of adding the mixed solution of (2-AET)X, organic halide and HI to the mixed solution of SnI2 and HI is 1 to 1.5 mL / min.
7. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The H3PO2 solution is prepared by mixing H3PO2 and deionized water, with a mass fraction of 50%; the molar ratio of HI to H3PO2 is 8 to 10:
1.
8. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The heating temperature is 90-120°C; the cooling rate is 3-3.5°C / h, and the crystallization time is 20-23h. The slow cooling operation can slow down the nucleation rate, resulting in fewer crystal nuclei, thereby obtaining larger crystals with full and regular grains.
9. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The slow dripping rate is 2-3 mL / min.
10. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: The drying temperature is 35-45° C. and the drying time is 25-35 minutes.
11. The method for preparing a cysteamine tin-based perovskite single crystal according to claim 1, characterized in that: All the steps are carried out in a nitrogen atmosphere with an oxygen content below 0.01 ppm.
Citation Information
Patent Citations
Perovskite work function regulator, perovskite solar cell and preparation method and application thereof
CN115768228A