Electronic grade meta-aramid fiber and preparation method thereof

By introducing melamine cyanate and modified semiconductor materials into meta-aramid fibers, the problem of insufficient thermal stability and electrical performance of electronic grade fibers in the prior art was solved, and excellent electrical resistance and low dielectric loss were prepared. Electronic grade mesoameric aramid fiber, suitable for high-end electronic cloth.

CN118727187BActive Publication Date: 2024-11-26TAYHO ADVANCED MATERIALS GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411222990.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing electronic-grade glass fibers are difficult to produce, have poor quality stability, and have poor electrical performance of meta-aramid fibers, with high dielectric constant and large dielectric loss, which limits the large-scale application of high-end electronic cloth in circuit boards.

Method used

The nucleophilic reaction is carried out by melamine cyanate and meta-aramid polymerization stock solution, combined with modified semiconductor materials, and electronic grade meta-aramid fibers are prepared by spinning to improve the thermal stability and electrical properties of the fibers.

Benefits of technology

The prepared electronic grade mesoameric fiber has excellent electrical resistance and thermal stability, with a dielectric constant of 1.4~1.6, and a dielectric loss of 0.2×10-3~0.4×10-3, which is suitable for high-end electronics. cloth application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727187B_ABST
    Figure CN118727187B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of electronic grade fiber materials, and in particular to an electronic grade meta-aramid fiber and a preparation method thereof. The preparation method comprises: uniformly dispersing melamine cyanate in an organic solvent to obtain an organic solution, then adding the organic solution to a meta-aramid polymer stock solution to react to obtain a meta-aramid melamine cyanate complex; fully homogenizing a modified semiconductor composite material and an organic solvent to obtain a modified material mixture, adding the modified material mixture to the meta-aramid melamine cyanate complex, and mixing uniformly to obtain an electronic grade meta-aramid polymer stock solution; spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber. The electronic grade meta-aramid fiber has reliable electrical properties while maintaining excellent mechanical properties, dimensional thermal stability, and fire retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to electronic grade meta-aramid fiber and a preparation method thereof, belonging to the technical field of electronic grade fiber materials. Background Art

[0002] In recent years, with the continuous development of 5G communication technology, my country has become the world's largest producer of electronic-grade fibers and the largest manufacturer of printed circuit boards. It is the world's largest electronic product production base and the world's major electronic product consumer market. The electronic cloth in the circuit board is used as a reinforcing material and is impregnated with adhesives composed of different resins to form a copper-clad laminate. As a common board in printed circuit boards, it is an important basic material for the electronics industry. The market application space of electronic cloth is determined by the markets in terminal fields such as communications, automotive electronics, and consumer electronics. In the 5G era, wireless signals will extend to higher frequency bands. Since the base station coverage area is inversely proportional to the communication frequency, the base station density and mobile data calculations will increase significantly.

[0003] At present, the main material of electronic cloth is electronic grade glass fiber, which is an inorganic fiber material with good insulation, strong heat resistance, good corrosion resistance and high mechanical strength. It is widely used in the field of circuit board electronic cloth. For example, Chinese patent applications CN115821574A and CN109797485A use glass fiber to make electronic cloth. However, due to the high brittleness, complex material composition and poor wear resistance of glass fiber, it is not conducive to the production and subsequent processing of the fiber. In addition, electronic glass fiber is a Class 2B carcinogen and there is a risk of endangering human physical and mental health during production and use.

[0004] Meta-aramid fiber is a special organic fiber material with the characteristics of high temperature resistance, flame retardancy, high strength and stable chemical properties. In addition, the fiber has a single composition and high flexibility in fiber modification, which provides conditions for fiber empowerment. However, meta-aramid currently has problems such as unsatisfactory dielectric constant, excessive dielectric loss and unsatisfactory thermal stability, and cannot be directly used in electronic cloth.

[0005] To sum up, among the existing fiber products, electronic-grade glass fiber is difficult to produce, the fiber quality stability is poor, the product safety is low, the electrical properties of meta-aramid fiber are not ideal, the dielectric constant is high, and the dielectric loss is large. These problems limit the large-scale application of high-end electronic cloth in circuit boards. Summary of the invention

[0006] The present invention aims at the deficiencies in the prior art and provides an electronic grade meta-aramid fiber and a preparation method thereof. The electronic grade meta-aramid fiber has good electrical resistance and thermal stability, and solves the problems of unsatisfactory electrical constants and excessive dielectric loss of conventional meta-aramid fibers.

[0007] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing electronic grade meta-aramid fiber, the preparation method comprising:

[0008] S1, uniformly dispersing melamine cyanate in an organic solvent to obtain an organic solution, and then adding the organic solution to a meta-aramid polymerization stock solution to react to obtain a meta-aramid melamine cyanate complex;

[0009] S2, fully homogenizing the modified semiconductor composite material and the organic solvent to obtain a modified material mixture, adding the modified material mixture to the meta-aramid melamine cyanate complex, and mixing them evenly to obtain an electronic grade meta-aramid polymerization stock solution;

[0010] The preparation method of the modified semiconductor composite material is as follows: adding the semiconductor material to a 5,6-dihydroxyindole reaction aqueous solution containing an oxidation promoter for in-situ modification, and then performing solid-liquid separation and drying to obtain the modified semiconductor composite material;

[0011] S3, spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber.

[0012] Furthermore, the organic solvent is any one of N,N-dimethylacetamide, N,N-dimethylformamide and N-methylpyrrolidone, or a mixture of two of them.

[0013] Further, the semiconductor material is any one of silicon carbide (SiC), gallium nitride (GaN) and diamond or a mixture of several thereof;

[0014] The oxidation promoter is at least one of a combination of CuSO4 and H2O2, (NH4)2S2O8, NaIO4, and KMnO4.

[0015] Furthermore, the reaction temperature of step S1 is 60-110° C., and the reaction time is 1-3 h;

[0016] In step S2, the temperature of the in-situ modification is 5-8°C.

[0017] Furthermore, the viscosity of the meta-aramid polymer stock solution is 200-500 Po; the weight average molecular weight of the polymer in the meta-aramid polymer stock solution is 10-14 W, and the mass ratio of the melamine cyanate to the meta-aramid polymer stock solution is 1:(10-16).

[0018] Furthermore, the mass ratio of the 5,6-dihydroxyindole to the semiconductor material is 1:(13-16); the dosage ratio of the 5,6-dihydroxyindole to deionized water is 1 g:(100-150) mL; the concentration of the oxidation promoter in the reaction aqueous solution is 13-18 mmol∙L-1 .

[0019] Further, in step S1, the mass concentration of melamine cyanate in the organic solution is 40%-50%;

[0020] In step S2, the mass ratio of the modified semiconductor composite material to the organic solvent is 1:(2-4), and the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:(20-25).

[0021] Furthermore, the preparation method of the meta-aramid polymer stock solution is: polymerize m-phenylenediamine and isophthaloyl chloride in an organic solvent, add isophthalic acid for end-capping, and after the reaction is completed, adjust the pH to 7-8 to obtain the meta-aramid polymer stock solution.

[0022] Furthermore, during the spinning process of step S3, the pump supply is 7-10 r / min; the spinning speed is 7-10 m / min;

[0023] The coagulation bath is a mixed solution of the organic solvent and water, the mass concentration of the organic solvent in the coagulation bath is 68% to 72%, and the temperature of the coagulation bath is 0° C. to 5° C.

[0024] The invention also discloses an electronic grade meta-aramid fiber, and the electronic grade meta-aramid fiber is prepared by adopting the preparation method of the invention.

[0025] The beneficial effects of the present invention are:

[0026] The carbonized nitrogen, gallium nitride and diamond in the electronic-grade meta-aramid fiber of the present invention have excellent electrical properties. In the preparation method of the present invention, melamine cyanate is used to react with the meta-aramid polymerization stock solution to carry out a nucleophilic reaction, so as to improve the thermal stability of the fiber body, and the meta-aramid melamine cyanate complex is compounded with the modified semiconductor material to obtain the electronic-grade meta-aramid fiber. The strength of the meta-aramid fiber is still maintained above 4.0 cN / dtex, the elongation at break is maintained above 30%, there is no obvious hair, the limiting oxygen index is greater than 30, the dielectric constant is 1.4-1.6, and the dielectric loss is 0.2×10 -3 ~0.4×10 -3 At the same time, using meta-aramid organic fiber as the main material is beneficial to combining with phenolic resin to prepare a circuit board composite material with more stable performance.

[0027] In the preparation method of the present invention, the meta-aramid fiber and melamine cyanate are compounded by certain reaction conditions (melamine cyanate organic solution is gradually added to the meta-aramid polymerization stock solution system under high temperature conditions to react, and melamine cyanate is grafted onto the polymer chain by nucleophilic addition reaction to obtain a meta-aramid fiber melamine cyanate complex), so that the meta-aramid fiber has electronic grade heat resistance, improves the thermal stability of the electronic cloth material, and further improves the operation stability of the circuit board.

[0028] The modified semiconductor composite material of the present invention performs in-situ modification of 5,6-dihydroxyindole on the surface of the semiconductor material, so that the surface of the semiconductor material has a large number of hydrogen bonds. The presence of a large number of hydrogen bonds enhances the interaction between the semiconductor material and the meta-aramid molecular chain, effectively solves the problem of large-scale precipitation of semiconductor materials during the fiber molding process, and improves the stability of the semiconductor material in the fiber matrix.

[0029] The electronic-grade meta-aramid fiber of the present invention exhibits low dielectric and low loss properties without damaging other properties of the fiber. The electronic modification of meta-aramid fiber is a form of multifunctionalization of meta-aramid fiber. Through the electronic modification process of meta-aramid fiber, the application of meta-aramid fiber in the field of electronic cloth becomes possible, which is a new application mode of meta-aramid fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a microscope picture of the fiber surface of the electronic grade meta-aramid fiber described in Example 1;

[0031] Figure 2 This is a microscope picture of the fiber surface of the electronic grade meta-aramid fiber described in Comparative Example 5. DETAILED DESCRIPTION

[0032] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.

[0034] A method for preparing electronic grade meta-aramid fiber, the preparation method comprising:

[0035] S1, uniformly dispersing melamine cyanate in an organic solvent to obtain an organic solution, and then adding the organic solution to a meta-aramid polymerization stock solution to react to obtain a meta-aramid melamine cyanate complex;

[0036] S2, fully homogenizing the modified semiconductor composite material and the organic solvent to obtain a modified material mixture, adding the modified material mixture to the meta-aramid melamine cyanate complex, and mixing them evenly to obtain an electronic grade meta-aramid polymerization stock solution;

[0037] The preparation method of the modified semiconductor composite material is as follows: adding the semiconductor material to a 5,6-dihydroxyindole reaction aqueous solution containing an oxidation promoter for in-situ modification, and then performing solid-liquid separation and drying to obtain a modified semiconductor composite material with a large number of hydrogen bonds;

[0038] S3, spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber.

[0039] Specifically, the organic solvent is any one of N,N-dimethylacetamide, N,N-dimethylformamide and N-methylpyrrolidone, or a mixture of two of them.

[0040] Specifically, in an embodiment of the present invention, the semiconductor material is any one of silicon carbide (powder with a particle size of 40 microns), gallium nitride (powder with a particle size of 40 microns) and diamond (powder with a particle size of 40 microns) or a mixture of several thereof;

[0041] The oxidation promoter is at least one of a combination of CuSO4 and H2O2, (NH4)2S2O8, NaIO4, and KMnO4.

[0042] Specifically, the reaction temperature of step S1 is 60-110° C., and the reaction time is 1-3 hours. Under high temperature conditions, the melamine cyanate organic solution is gradually added to the meta-aramid polymerization stock solution system for reaction, and the melamine cyanate is grafted onto the polymer chain through a nucleophilic addition reaction to obtain a meta-aramid melamine cyanate complex, which effectively improves the dimensional stability of the meta-aramid fiber under heating conditions.

[0043] Specifically, in step S2, the temperature of the in-situ modification is 5-8°C.

[0044] Specifically, the viscosity of the meta-aramid polymerization stock solution is 200-500 Po; the weight average molecular weight of the polymer in the meta-aramid polymerization stock solution is 10-14 W, and the mass ratio of the melamine cyanate to the meta-aramid polymerization stock solution is 1: (10-16).

[0045] Specifically, the mass ratio of the 5,6-dihydroxyindole to the semiconductor material is 1:(13-16); the dosage ratio of the 5,6-dihydroxyindole to deionized water is 1 g:(100-150) mL; the concentration of the oxidation promoter in the reaction aqueous solution is 13-18 mmol∙L -1 .

[0046] Specifically, in step S1, the mass concentration of melamine cyanate in the organic solution is 40%-50%;

[0047] In step S2, the mass ratio of the modified semiconductor composite material to the organic solvent is 1:(2-4), and the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:(20-25).

[0048] Specifically, the preparation method of the meta-aramid polymer stock solution is: meta-phenylenediamine and isophthaloyl chloride are polymerized in an organic solvent, and isophthalic acid is added for end-capping. After the reaction is completed, the pH is adjusted to 7-8 to obtain the meta-aramid polymer stock solution.

[0049] More specifically, the molar ratio of m-phenylenediamine to isophthaloyl chloride is 1:(0.85-0.95), and isophthalic acid is added for end-capping, and the molar ratio of m-phenylenediamine to isophthalic acid is 1:(0.05-0.15); the mass ratio of the total mass of m-phenylenediamine, isophthaloyl chloride and isophthalic acid to the mass ratio of the organic solvent is 1:(4-6).

[0050] Specifically, during the spinning process of step S3, the pump supply is 7-10 r / min; the spinning speed is 7-10 m / min; the spinneret aperture is 0.1-0.2 mm;

[0051] The coagulation bath is a mixture of the organic solvent and water, the mass concentration of the organic solvent in the coagulation bath is 68% to 72%, and the temperature of the coagulation bath is 0° C. to 5° C. Under the spinning conditions, the fibers can be formed more uniformly, reducing the phenomenon of decreased signal transmission stability due to excessive fiber hair.

[0052] Disclosed is an electronic grade meta-aramid fiber, which is prepared by adopting the preparation method of the present invention.

[0053] Example 1

[0054] Preparation of electronic grade meta-aramid fiber:

[0055] S1. Preparation of meta-aramid polymerization stock solution:

[0056] Meta-phenylenediamine and isophthaloyl chloride are polymerized in N,N-dimethylacetamide to obtain meta-aramid polymerization stock solution; wherein the molar ratio of meta-phenylenediamine to isophthaloyl chloride is 1:0.85, and isophthalic acid is added for end-capping, and the molar ratio of meta-phenylenediamine to isophthalic acid is 1:0.15; the total mass ratio of meta-phenylenediamine, isophthaloyl chloride and isophthalic acid to the mass ratio of organic solvent is 1:6, the reaction temperature is 5°C, and after the reaction is completed, ammonia is used to adjust the pH to 7 to obtain the meta-aramid polymerization stock solution; the viscosity of the meta-aramid polymerization stock solution is 220 Po.

[0057] S2, meta-aramid melamine cyanate complex:

[0058] Melamine cyanate is fully homogenized in N,N-dimethylacetamide to obtain a melamine cyanate organic solution with a mass fraction of 50%. The melamine cyanate organic solution is gradually added into a meta-aramid polymerization stock solution system at 100°C for reaction for 2 hours, and melamine cyanate is grafted onto a polymer chain through a nucleophilic addition reaction to obtain a meta-aramid melamine cyanate complex.

[0059] The mass ratio of the melamine cyanate organic solution to the meta-aramid polymerization stock solution is 1:10.

[0060] S3. Preparation of surface hydroxyl-modified diamond composite material:

[0061] 5,6-dihydroxyindole and diamond were added to deionized water containing (NH4)2S2O8 for in-situ modification, shaken at 5°C for 4 hours to complete the modification treatment, and then the solid-liquid separation was carried out by centrifuge. The separated solid was then washed three times with a 25wt.% isopropanol aqueous solution; then vacuum dried at 40-50°C to obtain surface hydroxyl-modified diamond; the mass ratio of 5,6-dihydroxyindole to semiconductor material was 1:13; the dosage ratio of 5,6-dihydroxyindole to deionized water was 1g:100mL; the concentration of (NH4)2S2O8 in the modified solution was 13 mmol∙L -1 .

[0062] S4, mixing the surface hydroxyl-modified diamond composite material with N,N-dimethylacetamide (DMAC) by high-speed shearing, and then using high-pressure blasting nanomaterial dispersion technology to fully homogenize the surface hydroxyl-modified diamond in the DMAC solvent system to obtain a modified material mixture, and uniformly mixing the modified material mixture with the meta-aramid melamine cyanate complex to obtain an electronic grade meta-aramid polymerization stock solution;

[0063] Among them, the mass ratio of the surface hydroxyl-modified diamond composite material to DMAC is 1:2; the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:25.

[0064] S5. Preparation of electronic grade meta-aramid fiber: spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber; during the spinning process, the coagulation bath is a mixture of N,N-dimethylacetamide and water, the mass concentration of N,N-dimethylacetamide in the coagulation bath is 68%, the coagulation bath temperature is 2°C, the pump supply is 7r / min, the spinning speed is 7m / min, and the spinneret aperture is 0.1mm.

[0065] Example 2

[0066] Preparation of electronic grade meta-aramid fiber:

[0067] S1. Preparation of meta-aramid polymerization stock solution:

[0068] Metaphenylenediamine and isophthaloyl chloride are polymerized in N,N-dimethylformamide to obtain a meta-aramid polymerization stock solution; the molar ratio of the metaphenylenediamine to isophthaloyl chloride is 1:0.9, and isophthalic acid is added for end-capping, and the molar ratio of the metaphenylenediamine to isophthalic acid is 1:0.1; the total mass ratio of the metaphenylenediamine, isophthaloyl chloride and isophthalic acid to the mass ratio of the organic solvent is 1:5, the reaction temperature is 10°C, and after the reaction is completed, ammonia is used to adjust the pH to 8 to obtain the meta-aramid polymerization stock solution; the viscosity of the meta-aramid polymerization stock solution is 238 Po.

[0069] S2, meta-aramid melamine cyanate complex:

[0070] Melamine cyanate is fully homogenized in an organic solvent, N,N-dimethylformamide, to obtain a melamine cyanate organic solution with a mass fraction of 50%. The melamine cyanate organic solution is gradually added into a meta-aramid polymerization stock solution system at 110°C for reaction for 1.5 hours. Melamine cyanate is grafted onto a polymer chain through a nucleophilic addition reaction to obtain a meta-aramid melamine cyanate complex.

[0071] The mass ratio of the melamine cyanate organic solution to the meta-aramid polymerization stock solution is 1:10.

[0072] S3. Preparation of surface hydroxyl-modified diamond composite material:

[0073] 5,6-dihydroxyindole and diamond were added to deionized water containing NaIO4 for in-situ modification, shaken at 6°C for 4 hours to complete the modification treatment, and then the solid-liquid separation was carried out by centrifuge, and the separated solid was washed 3 times with 25wt.% isopropanol aqueous solution; then vacuum dried at 40-50°C to obtain surface hydroxyl-modified diamond; the mass ratio of 5,6-dihydroxyindole to semiconductor material was 1:15; the dosage ratio of 5,6-dihydroxyindole to deionized water was 1g:120mL; the concentration of NaIO4 in the modified solution was 15 mmol∙L -1 .

[0074] S4, high-speed shear mixing of the surface hydroxyl-modified diamond composite material and N,N-dimethylformamide, and then high-pressure blasting nanomaterial dispersion technology to fully homogenize the surface hydroxyl-modified diamond in the N,N-dimethylformamide solvent system to obtain a modified material mixture, and the modified material mixture is evenly mixed with the meta-aramid melamine cyanate complex to obtain an electronic grade meta-aramid polymerization stock solution;

[0075] The mass ratio of the surface hydroxyl-modified diamond composite material to N,N-dimethylformamide is 1:2; the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:20.

[0076] S5. Preparation of electronic-grade meta-aramid fiber: spinning the electronic-grade meta-aramid polymer stock solution to obtain the electronic-grade meta-aramid fiber; during the spinning process, the coagulation bath is a mixture of N,N-dimethylformamide and water, the mass concentration of N,N-dimethylformamide in the coagulation bath is 70%, the coagulation bath temperature is 4°C, the pump supply is 8r / min, the spinning speed is 8m / min, and the spinneret aperture is 0.1mm.

[0077] Example 3

[0078] Preparation of electronic grade meta-aramid fiber:

[0079] S1. Preparation of meta-aramid polymerization stock solution:

[0080] Meta-phenylenediamine and isophthaloyl chloride are polymerized in N-methylpyrrolidone to obtain a meta-aramid polymerization stock solution; the molar ratio of the meta-phenylenediamine to isophthaloyl chloride is 1:0.95, and isophthalic acid is added for end-capping, and the molar ratio of the meta-phenylenediamine to isophthalic acid is 1:0.05; the mass ratio of the total mass of meta-phenylenediamine, isophthaloyl chloride and isophthalic acid to the mass ratio of the organic solvent is 1:4, the reaction temperature is 0°C, and after the reaction is completed, ammonia is used to adjust the pH to 7 to obtain the meta-aramid polymerization stock solution; the viscosity of the meta-aramid polymerization stock solution is 310 Po.

[0081] S2, meta-aramid melamine cyanate complex:

[0082] Melamine cyanate was fully homogenized in an organic solvent of N-methylpyrrolidone to obtain a melamine cyanate organic solution with a mass fraction of 50%. The melamine cyanate organic solution was gradually added into a meta-aramid polymerization stock solution system at 60°C for reaction for 3 hours. Melamine cyanate was grafted onto a polymer chain through a nucleophilic addition reaction to obtain a meta-aramid melamine cyanate complex.

[0083] The mass ratio of the melamine cyanate organic solution to the meta-aramid polymerization stock solution is 1:10.

[0084] S3. Preparation of surface hydroxyl-modified diamond composite material:

[0085] 5,6-dihydroxyindole and diamond were added to deionized water containing KMnO4 for in-situ modification, shaken at 8°C for 4 hours to complete the modification treatment, and then the solid-liquid separation was carried out by centrifuge, and the separated solid was washed 3 times with 25wt.% isopropanol aqueous solution; then vacuum dried at 40-50°C to obtain surface hydroxyl-modified diamond; the mass ratio of 5,6-dihydroxyindole to semiconductor material was 1:16; the dosage ratio of 5,6-dihydroxyindole to deionized water was 1g:150mL; the concentration of KMnO4 in the modified solution was 17 mmol∙L -1 .

[0086] S4, high-speed shear mixing of the surface hydroxyl-modified diamond composite material and N-methylpyrrolidone, and then high-pressure blasting nanomaterial dispersion technology to fully homogenize the surface hydroxyl-modified diamond in the N-methylpyrrolidone solvent system to obtain a modified material mixture, and the modified material mixture is evenly mixed with the meta-aramid melamine cyanate complex to obtain an electronic grade meta-aramid polymerization stock solution;

[0087] Among them, the mass ratio of the surface hydroxyl-modified diamond composite material to N-methylpyrrolidone is 1:3; the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:20.

[0088] S5. Preparation of electronic-grade meta-aramid fiber: spinning the electronic-grade meta-aramid polymer stock solution to obtain the electronic-grade meta-aramid fiber; during the spinning process, the coagulation bath is a mixture of N-methylpyrrolidone and water, the mass concentration of N-methylpyrrolidone in the coagulation bath is 72%, the coagulation bath temperature is 5°C, the pump supply is 10r / min, the spinning speed is 10m / min, and the spinneret aperture is 0.1mm.

[0089] Example 4

[0090] Preparation of electronic grade meta-aramid fiber:

[0091] S1. Preparation of meta-aramid polymerization stock solution:

[0092] Meta-phenylenediamine and isophthaloyl chloride are polymerized in N-methylpyrrolidone to obtain a meta-aramid polymerization stock solution; the molar ratio of the meta-phenylenediamine to isophthaloyl chloride is 1:0.95, and isophthalic acid is added for end-capping, and the molar ratio of the meta-phenylenediamine to isophthalic acid is 1:0.05; the total mass ratio of the meta-phenylenediamine, isophthaloyl chloride and isophthalic acid to the mass ratio of the organic solvent is 1:4, the reaction temperature is 5°C, and after the reaction is completed, ammonia is used to adjust the pH to 7 to obtain the meta-aramid polymerization stock solution; the viscosity of the meta-aramid polymerization stock solution is 302 Po.

[0093] S2, meta-aramid melamine cyanate complex:

[0094] Melamine cyanate was fully homogenized in an organic solvent of N-methylpyrrolidone to obtain a 40% by mass melamine cyanate organic solution, which was gradually added into a meta-aramid polymerization stock solution system at 90°C for reaction for 1.5 hours, and melamine cyanate was grafted onto a polymer chain through a nucleophilic addition reaction to obtain a meta-aramid melamine cyanate complex.

[0095] The mass ratio of the melamine cyanate organic solution to the meta-aramid polymerization stock solution is 1:13.

[0096] S3. Preparation of surface hydroxyl-modified silicon carbide composite material:

[0097] 5,6-dihydroxyindole and silicon carbide were added to deionized water containing KMnO4 for in-situ modification, shaken at 6°C for 4 hours to complete the modification treatment, and then the solid-liquid separation was carried out by centrifuge, and the separated solid was washed 3 times with 25wt.% isopropanol aqueous solution; then vacuum dried at 40-50°C to obtain surface hydroxyl-modified silicon carbide; the mass ratio of 5,6-dihydroxyindole to silicon carbide was 1:15; the dosage ratio of 5,6-dihydroxyindole to deionized water was 1g:120mL; the concentration of KMnO4 in the modified solution was 18 mmol∙L -1 .

[0098] S4, subjecting the surface hydroxyl-modified silicon carbide composite material to high-speed shear mixing with N-methylpyrrolidone, and then subjecting the surface hydroxyl-modified silicon carbide composite material to high-pressure blasting nanomaterial dispersion technology, so that the surface hydroxyl-modified silicon carbide composite material is fully homogenized in the N-methylpyrrolidone solvent system to obtain a modified material mixture, and the modified material mixture is evenly mixed with the meta-aramid melamine cyanate complex to obtain an electronic grade meta-aramid polymerization stock solution;

[0099] Among them, the mass ratio of the surface hydroxyl-modified silicon carbide composite material to N-methylpyrrolidone is 1:2; the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:20.

[0100] S5. Preparation of electronic grade meta-aramid fiber: spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber; during the spinning process, the coagulation bath is a mixture of N-methylpyrrolidone and water, the mass concentration of N-methylpyrrolidone in the coagulation bath is 70%, the coagulation bath temperature is 2°C, the pump supply is 8r / min, the spinning speed is 8m / min, and the spinneret aperture is 0.1mm.

[0101] Example 5

[0102] Preparation of electronic grade meta-aramid fiber:

[0103] S1. Preparation of meta-aramid polymerization stock solution:

[0104] Metaphenylenediamine and isophthaloyl chloride are polymerized in N,N-dimethylformamide to obtain a meta-aramid polymerization stock solution; the molar ratio of the metaphenylenediamine to isophthaloyl chloride is 1:0.9, and isophthalic acid is added for end-capping, and the molar ratio of the metaphenylenediamine to isophthalic acid is 1:0.08; the total mass ratio of the metaphenylenediamine, isophthaloyl chloride and isophthalic acid to the mass ratio of the organic solvent is 1:5, the reaction temperature is 8°C, and after the reaction is completed, ammonia is used to adjust the pH to 7 to obtain the meta-aramid polymerization stock solution; the viscosity of the meta-aramid polymerization stock solution is 243 Po.

[0105] S2, meta-aramid melamine cyanate complex:

[0106] Melamine cyanate is fully homogenized in an organic solvent of N,N-dimethylformamide to obtain a melamine cyanate organic solution with a mass fraction of 50%. The melamine cyanate organic solution is gradually added into a meta-aramid polymerization stock solution system at 100°C for reaction for 1.5 hours. Melamine cyanate is grafted onto a polymer chain through a nucleophilic addition reaction to obtain a meta-aramid melamine cyanate complex.

[0107] The mass ratio of the melamine cyanate organic solution to the meta-aramid polymerization stock solution is 1:16.

[0108] S3. Preparation of surface hydroxyl-modified gallium nitride composite material:

[0109] 5,6-dihydroxyindole and gallium nitride were added to deionized water containing KMnO4 for in-situ modification, shaken at 5°C for 4 hours to complete the modification treatment, and then the solid-liquid separation was performed by a centrifuge. The separated solid was then washed three times with a 25wt.% isopropanol aqueous solution; then vacuum dried at 40-50°C to obtain surface hydroxyl-modified gallium nitride; the mass ratio of 5,6-dihydroxyindole to gallium nitride was 1:14; the dosage ratio of 5,6-dihydroxyindole to deionized water was 1g:110mL; the concentration of KMnO4 in the modified solution was 15 mmol∙L -1 .

[0110] S4, high-speed shear mixing of the surface hydroxyl-modified gallium nitride composite material and N,N-dimethylformamide, and then high-pressure blasting nanomaterial dispersion technology to fully homogenize the surface hydroxyl-modified silicon carbide composite material in the N,N-dimethylformamide solvent system to obtain a modified material mixture, and the modified material mixture is evenly mixed with the meta-aramid melamine cyanate complex to obtain an electronic grade meta-aramid polymerization stock solution;

[0111] Among them, the mass ratio of the surface hydroxyl-modified gallium nitride composite material to N,N-dimethylformamide is 1:4; the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:25.

[0112] S5. Preparation of electronic grade meta-aramid fiber: spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber; during the spinning process, the coagulation bath is a mixture of N,N-dimethylformamide and water, the mass concentration of N,N-dimethylformamide in the coagulation bath is 68%, the coagulation bath temperature is 3°C, the pump supply is 9r / min, the spinning speed is 9m / min, and the spinneret aperture is 0.1mm.

[0113] Comparative Example 1

[0114] Electronic grade meta-aramid fiber was prepared by the same method as in Example 1, except that: in this comparative example 1, no meta-aramid melamine cyanate complex was prepared, that is, step S2 was not performed, and melamine cyanate was not added in step S2; in step S4, the modified material mixture and the meta-aramid polymerization stock solution were directly mixed evenly.

[0115] Comparative Example 2

[0116] Electronic grade meta-aramid fiber was prepared by the same method as in Example 1, except that: in this comparative example 2, step S3 was not performed; that is, the hydroxyl groups on the diamond surface were not modified, and in step S4, the unmodified diamond was directly mixed evenly with the meta-aramid melamine cyanate complex.

[0117] Comparative Example 3

[0118] The electronic grade meta-aramid fiber was prepared by the same method as in Example 1, except that in Comparative Example 3, no semiconductor material was added to the meta-aramid melamine cyanate complex, that is, steps S3 and S4 were not performed.

[0119] Comparative Example 4

[0120] Electronic grade meta-aramid fiber was prepared by the same method as in Example 1, except that: in step S2 of this comparative example 4, no nucleophilic reaction was performed under heating conditions, and 50% melamine cyanate organic solution was directly added to the meta-aramid polymerization stock solution.

[0121] Comparative Example 5

[0122] Electronic grade meta-aramid fiber was prepared by the same method as in Example 1, except that: step S5 adopted a conventional spinning process, the coagulation bath concentration was 65%, the coagulation bath temperature was 15°C, the pump supply was 20 r / min, and the spinning speed was 20 m / min.

[0123] Blank example

[0124] The aramid stock solution was prepared by the same method as step S1 of Example 1, and then the aramid fiber was prepared by spinning by the same method as step S5 of Example 1.

[0125] The performance tests were conducted on the aramid fibers prepared in the above Examples 1-5, Comparative Examples 1-5 and Blank Examples. The specific test data are shown in Table 1 below. The relevant test methods are as follows:

[0126] (1) Thermal shrinkage test method:

[0127] ①Put the test sample on the flannel board, take out a fiber with tweezers, carefully clamp the fiber at the lower end with a tension clamp, and pre-apply a tension of 100 mg;

[0128] ② Make two marks at both ends of the above-mentioned fiber, with the length between the two marks being 20-30cm. Use tweezers to hang the fiber and use a ruler to measure the vertical length L0 between the two marks, accurate to 1mm;

[0129] ③Put the sample into a weighing bottle and quickly put it into an oven heated to 300℃. When the oven temperature returns to 300℃, start recording the heat treatment time, which is 15 minutes.

[0130] ④After dry heat treatment, carefully take out the sample and equilibrate it in air for 15 minutes;

[0131] ⑤ Use a ruler to measure the vertical length L1 of the two marks again;

[0132] ⑥Result calculation

[0133] Shrinkage calculation formula

[0134] S=(L0-L1) / L0×100%

[0135] Where: S is the dry heat shrinkage rate, unit: %

[0136] L0 is the length of the sample before heat treatment, in mm;

[0137] L1 is the length of the sample after heat treatment, in mm.

[0138] Calculate to two decimal places and round to one decimal place according to GB / T 8170.

[0139] (2) Electrical performance test method: Test according to IEC61189-2-721-2015.

[0140] (3) Test method for fiber breaking strength performance: Test according to GB / T 14337-2008 test method.

[0141] (4) Flame retardant performance test method: Test according to GB17591-2006 GB20286-2006 test method.

[0142] (5) Thermal expansion coefficient test method: Test according to national standard GB / T1039-2008.

[0143] Table 1 Performance data of electronic grade meta-aramid fiber

[0144]

[0145] It can be seen from the data in Table 1 that the electronic-grade meta-aramid fibers prepared by the preparation method of the present invention in Examples 1-3 have excellent electrical properties, and the meta-fiber strength is still maintained above 4.0 cN / dtex, the elongation at break is maintained above 30%, and the limiting oxygen index is greater than 30. At the same time, it also has good thermal stability and chemical stability and other properties, which can meet the needs of different application scenarios.

[0146] From the comparison of the data of Comparative Example 1 and Example 1, it can be seen that if melamine cyanate is not introduced into the meta-aramid fiber, the thermal stability of the fiber is much worse than the thermal stability of the fiber product prepared in Example 1, which will cause the dimensional stability of the electronic cloth to deteriorate under high-power working conditions, thereby affecting the transmission stability of the electrical signal.

[0147] From the comparison of the data of Comparative Example 2 and Example 1, it can be seen that if the semiconductor material without surface hydroxyl modification is directly added to the meta-aramid polymerization stock solution, the dielectric properties of the meta-aramid will be significantly reduced. This is because the bonding force between the semiconductor material and the fiber body is reduced, most of the semiconductor material is precipitated from the fiber system during the spinning process, the semiconductor content in the fiber is reduced and the distribution is uneven, which manifests as a substantial attenuation of the dielectric properties of the fiber.

[0148] From the data comparison between Comparative Example 3 and Example 1, it can be seen that if no semiconductor material is added to the composite system, the dielectric properties of the meta-aramid fiber will deteriorate, the dielectric constant will reach 4.01, and the dielectric loss will reach 1.95×10 -3 , it will not be able to meet the application requirements of meta-aramid fiber in the field of 5G electronic cloth (dielectric constant 2.8~3.2).

[0149] From the comparison of the data of Comparative Example 4 and Example 1, it can be seen that if the meta-aramid melamine cyanate composite is not prepared and the two are directly physically mixed, the melamine cyanate will precipitate during the spinning process, which will lead to the deterioration of the heat resistance of the meta-aramid fiber, the dry heat shrinkage rate reaches 2.45%, and the thermal expansion coefficient reaches 10.3×10 -6 , the dielectric constant and dielectric loss are improved.

[0150] From the comparison of the data of Comparative Example 5 and Example 1, it can be seen that if the spinning process is not carried out according to the spinning process defined in the present invention, the hairiness of the meta-aramid fiber will increase (by Figure 1 and Figure 2 It can be clearly seen in the microscope picture of the ), which in turn affects the dielectric properties. The dielectric constant reaches 4.11 and the dielectric loss reaches 2.12×10 -3 , it will not be able to meet the application requirements of meta-aramid fiber in the field of 5G electronic cloth (dielectric constant 2.8~3.2).

[0151] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0152] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for preparing electronic grade meta-aramid fiber, characterized in that: The preparation method is: S1, uniformly dispersing melamine cyanate in an organic solvent to obtain an organic solution, and then adding the organic solution to a meta-aramid polymerization stock solution to react to obtain a meta-aramid melamine cyanate complex; S2, fully homogenizing the modified semiconductor composite material and the organic solvent to obtain a modified material mixture, adding the modified material mixture to the meta-aramid melamine cyanate complex, and mixing them evenly to obtain an electronic grade meta-aramid polymerization stock solution; The preparation method of the modified semiconductor composite material is as follows: adding the semiconductor material to a 5,6-dihydroxyindole reaction aqueous solution containing an oxidation promoter for in-situ modification, and then performing solid-liquid separation and drying to obtain the modified semiconductor composite material; S3, spinning the electronic grade meta-aramid polymer stock solution to obtain the electronic grade meta-aramid fiber; The semiconductor material is any one of silicon carbide, gallium nitride and diamond or a mixture of several thereof; The oxidation promoter is at least one of a combination of CuSO4 and H2O2, (NH4)2S2O8, NaIO4, and KMnO4; The reaction temperature of step S1 is 60-110°C, and the reaction time is 1-3h; In step S2, the temperature of the in-situ modification is 5-8°C; During the spinning process of step S3, the pump supply is 7-10 r / min; the spinning speed is 7-10 m / min; The coagulation bath is a mixed solution of the organic solvent and water, the mass concentration of the organic solvent in the coagulation bath is 68% to 72%, and the temperature of the coagulation bath is 0° C. to 5° C.

2. The method for preparing electronic grade meta-aramid fiber according to claim 1, characterized in that: The organic solvent is any one of N,N-dimethylacetamide, N,N-dimethylformamide and N-methylpyrrolidone or a mixture of two of them.

3. The method for preparing electronic grade meta-aramid fiber according to claim 1, characterized in that: The viscosity of the meta-aramid polymerization stock solution is 200-500 Po; the weight average molecular weight of the polymer in the meta-aramid polymerization stock solution is 10-14W, and the mass ratio of the melamine cyanate to the meta-aramid polymerization stock solution is 1:(10-16).

4. The method for preparing electronic grade meta-aramid fiber according to claim 1, characterized in that: The mass ratio of the 5,6-dihydroxyindole to the semiconductor material is 1:(13-16); the dosage ratio of the 5,6-dihydroxyindole to deionized water is 1 g:(100-150) mL; the concentration of the oxidation promoter in the reaction aqueous solution is 13-18 mmol∙L -1 .

5. The method for preparing electronic grade meta-aramid fiber according to claim 1, characterized in that: In step S1, the mass concentration of melamine cyanate in the organic solution is 40%-50%; In step S2, the mass ratio of the modified semiconductor composite material to the organic solvent is 1:(2-4), and the mass ratio of the homogenized modified material mixture to the meta-aramid polymerization stock solution is 1:(20-25).

6. The method for preparing electronic grade meta-aramid fiber according to claim 1, characterized in that: The preparation method of the meta-aramid polymer stock solution is as follows: meta-phenylenediamine and isophthaloyl chloride are polymerized in an organic solvent, isophthalic acid is added for end-capping, and after the reaction is completed, the pH is adjusted to 7-8 to obtain the meta-aramid polymer stock solution.

7. An electronic grade meta-aramid fiber, characterized in that: The electronic grade meta-aramid fiber is prepared according to the preparation method according to any one of claims 1-6.

Citation Information

Cited By

  • A method for preparing a modified meta-aramid fibrid

    CN122727974A