Preparation process and method of double-layer composite burnt-out jean fabric

Through the preparation process of double-layer composite burnt denim fabric, the double-layer structure and acid spray baking technology are used to solve the problems of incomplete structure and tattered edges of denim fabric during burnt treatment, and achieve the thickness and wear resistance of the fabric. , significantly improving the durability and washability of the pattern.

CN118727233APending Publication Date: 2024-10-01河南新润纺织有限公司

Patent Information

Application Number
CN202411042674.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When existing denim fabrics are burned or laser hollowed out, it is easy to cause incomplete fabric structure, tattered edges and irreversible deformation. Moreover, the inner lining method cannot show the hollowing effect, which increases the difficulty of construction.

Method used

Using the preparation process of double-layer composite burnt denim fabric, through dyeing, weaving and finishing treatment, using the different dyeing and let-off ratios of the surface warp yarn and the inner warp yarn, combined with the weaving method of composite tissue and joint tissue, a double-layer structure is formed. Acid spraying and baking treatments are used to create hole-in-the-wall patterns, and a nylon bottom layer is used to increase the durability of the patterns.

Benefits of technology

It achieves the thickness and dimensional stability of the fabric, improves the sturdiness and wear resistance of the pattern, prevents irreversible deformation, and significantly improves the wear resistance and washability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727233A_ABST
    Figure CN118727233A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process and method of a double-layer composite burnt-out jean fabric. The preparation process comprises the following steps of dyeing, weaving and post-finishing treatment. The surface warp yarns B1 are subjected to warping (warp arrangement), dyeing, sizing, drying and drafting, then the surface warp yarns B1, the inner warp yarns A1, the surface weft yarns B2 and the inner weft yarns A2 are subjected to machine weaving, then after-finishing treatment is carried out, finished fabric is obtained, and the finished fabric is subjected to burn-out treatment to form holes; in the warping process, the surface warp B1 and the inner warp A1 are longitudinally arranged and wound on two warp beams respectively, the warp beam of the inner warp A1 is a line shaft, the warp beam of the surface warp B1 is an earth shaft, the surface warp B1 arranged on the earth shaft is dyed, and the let-off ratio of the inner warp A1 to the surface warp B1 is 2: 1; through the double-layer structure texture, the fabric is thick and solid, the size is stable, patterns are formed on the surface of the denim fabric through the later burn-out treatment, and through the nylon fabric on the bottom layer, the firmness and durability of the patterns are improved, irreversible deformation around the patterns is prevented, and the wear resistance and the washability can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of woven fabrics, and in particular relates to a preparation process and method of a double-layer composite burnt-out denim fabric. Background Art

[0002] The global production of denim exceeds 2 billion meters, with air-spun or ring-spun yarns. Currently, the main products are weft stretch denim, warp stretch denim or warp-weft bi-directional stretch denim; people are constantly developing denim with fashionable changes, and obtain novel appearance, feel and performance through dyeing and finishing.

[0003] Research continues into changing the look of denim through various chemical treatments and the use of effects such as flocking, embroidery and coatings. Other products developed include indigo-dyed jacquards, woven or knitted linen and cotton, laser cutouts on denim, matte sheen patterns and more personalised products.

[0004] During the weaving process of denim fabric, a single-layer weaving method is generally used. When burning or laser hollowing is performed, all of the fabric needs to be hollowed out, or the inner layer needs to be lined. Hollowing out all of the fabric will affect the integrity of the overall fabric structure of the clothes, and affect the strength and durability of the clothes. The hollowed-out edges are prone to tearing and forming irreversible deformation. The method of adding an inner layer lining not only increases the difficulty of construction, but also cannot produce a visual hollowing effect. Therefore, a new process and method are needed to solve the above problems. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a preparation process and method of a double-layer composite burnt-out denim fabric, which at least solves one of the problems of the background technology.

[0006] The present invention provides the following technical solutions:

[0007] A preparation process of a double-layer composite burnt-out denim fabric, a preparation process of a double-layer composite burnt-out denim fabric, characterized in that it comprises the following steps: dyeing, weaving, and post-processing; the surface warp yarn B1 is warped (warp arrangement), dyed, sizing, dried, and drawn into the weft, and then woven with the inner warp yarn A1, the surface weft yarn B2, and the inner weft yarn A2 on a machine, and then subjected to post-processing to obtain a finished fabric, and the finished fabric is subjected to a burnt-out process to form holes;

[0008] During the warp arrangement process, the outer warp yarn B1 and the inner warp yarn A1 are longitudinally arranged and wound on two warp beams, the warp beam of the inner warp yarn A1 is the sky beam, and the warp beam of the outer warp yarn B1 is the ground beam. The outer warp yarn B1 arranged on the ground beam is dyed, and the inner warp yarn A1 arranged on the sky beam is not dyed. The warp let-off ratio of the inner warp yarn A1: the outer warp yarn B1 is 2:1.

[0009] The outer weft yarn A2 and the inner weft yarn B2 are not dyed, and the warp ratio of the outer weft yarn A2: the inner weft yarn B2 is 1:2;

[0010] The warp drawing adopts 12-page heald frame, among which the 2nd, 3rd, 5th, 6th, 8th, 9th, 11th and 12th pages are drawn through the inner warp yarn A1 on the sky axis, and the 1st, 4th, 7th and 10th pages are drawn through the surface warp yarn B1 on the ground axis. The side weave is 1st and 2nd pages, and the ground weave is 3rd, 4th, 5th, 6th, 7th, 8th, 9th, 10th, 11th and 12th pages, and the ground weave is reversely drawn.

[0011] The heald lifting method adopts the weaving method of composite structure + combined structure: 1 up and 1 down + 2 up and 1 down.

[0012] The inner warp yarn A1 and the inner weft yarn B2 are made of nylon yarn; the outer warp yarn B1 and the outer weft yarn A2 are made of plain yarn.

[0013] Preferably, during the warping process, the total number of warp roots of the inner warp yarn A1 is 4339; the total number of warp roots of the outer warp yarn B1 is 3380, and the total number of warp roots is 7719; and the wheelbase of the warp beam is 190 cm.

[0014] Preferably, the length of the outer weft yarn A2 accounts for 33.33% of the total weft yarn length, and the yarn consumption per kilometer of the grey cloth is 134.95 kg; the length of the inner weft yarn B2 accounts for 66.67% of the total weft yarn length, and the yarn consumption per kilometer of the grey cloth is 30.89 kg.

[0015] Preferably, the reed number in the drawing-in process is 91#, the reed width is 185.7 cm, the number of yarns for the edge tissue is 40+40; the number of warp threads of the ground tissue is 3, the number of warp threads of the edge tissue is 2; the weft density on the machine is 105.

[0016] Preferably, in the dyeing process of the surface warp yarn B1, the plain yarn is used as the raw material, and is first subjected to a refining treatment, the refining agent is an alkyl alcohol polyoxyethylene ether fatty acid ester as the main component, the concentration is 4.5-5.5g / L, the refining temperature is 75°C, and the refining treatment is one time; after the yarn is subjected to the refining treatment, it is then subjected to three water washings, and the residual refining agent on the yarn is sprayed with clean water to remove the residual refining agent on the yarn, and then the yarn is dyed by a dyeing machine, and the speed of the dyeing machine is 21m / min; the dyeing temperature is 25-28°C, and the dye liquor is It comprises indigo, caustic soda and insurance powder, with a weight ratio of indigo: caustic soda: insurance powder of 1:1:1.2, and a caustic soda concentration of 100-150g / L; indigo is an aqueous indigo fuel with a concentration of 80-110g / L; the insurance powder is sodium dithionite with a concentration of 1.5-2.5g / L; 50g / L of the above ingredients are added during the dyeing process, and the concentration of the additional dye solution is 1.5g / L. After dyeing, the dye is washed with water at a water temperature of 50-70℃, with three washes and a washing time of 30-40min.

[0017] Preferably, during the dyeing process, a biological softener is added, which contains silk protein essence at a concentration of 2.5-3.5 g / L, and the softening treatment temperature is 50°C.

[0018] Preferably, the post-treatment includes singeing, desizing, washing, drying and pre-shrinking; singeing on both sides once, the singeing speed is 110m / min, desizing uses desizing enzyme with a concentration of 1g / L and penetrant with a concentration of 1g / L, desizing temperature is 60°C, and desizing vehicle speed is 55m / min; eight-slot desizing, water temperature is 55-65°C; pre-shrinking temperature is 135-150°C, warp and weft shrinkage is 1%-4%, and the finished cloth has a warp density of 172 and a weft density of 120.

[0019] Preferably, when the fabric is burned, the acid is dissolved in the paste and sprayed on the grey cloth to form the required pattern, and then the grey cloth is baked at a high temperature of 120-130°C for 2 to 3 minutes, and steamed at 95-97°C for 3 to 5 minutes; the surface warp yarn B1 and the surface weft yarn B2 at the spraying location are made of pure cotton, the water is evaporated, the acid concentration increases, the surface warp yarn B1 and the surface weft yarn B2 fibers are carbonized to become hydrated fibers with low polymerization degree and hydrolyzed to form a hole pattern; the inner warp yarn A1 and the inner weft yarn A2 are made of nylon and will not be carbonized, and the bottom of the hole pattern is a nylon mesh structure.

[0020] Preferably, the acid is dilute sulfuric acid with a concentration of 4.5%-6%; the paste is a mixed paste including white dextrin, dragon glue: emulsified paste with a weight ratio of 1:1:1 and a concentration of 60%-70%.

[0021] Preferably, the pre-shrinking process of the grey cloth adopts a short-machine double-shrinking method, in which the grey cloth passes through two sets of rubber blankets and is not connected to a mercerizing machine before pre-shrinking.

[0022] In addition, the inner warp yarn A1 and the inner weft yarn A2 use nylon line model Jinliyuan-N50+20D-non-Lycra 2.5 times, the surface warp yarn B1 uses flat yarn model Xinyize-C9, and the surface warp yarn B2 uses flat yarn model Tianhong-C12.

[0023] Preferably, the inner warp yarn A1 and the inner weft yarn A2 are made of nylon line model Jinliyuan-N50+30D-non-Lycra 2.5 times, and the amount of the inner warp yarn A1 is 3700 yarns.

[0024] The warp drawing length is 250 meters; the warp yarn is wrapped in the warping process, and the yarn is fixed by winding. Because nylon yarn is thin, it is warped by a small tension. The dynamic tension of the warping creel is 25-30CN, the pressure of the pressure roller is 100-200N, and the warping speed is 400-450r / min, so as to achieve the purpose of yarn flatness. In the warping process, the warp setting is simultaneously not twisted with the adjacent yarn. In the dyeing process, reduce chemical additives, use biological additives that do not damage the yarn to achieve the dyeing effect.

[0025] The loom parameters used are: heald frame height 123mm; opening time: 26°; back beam height 4cm; back beam depth: 4cm; warp stop frame height: -8cm; warp stop depth: 8cm; machine speed 400-450m / min; palm flat time: 308-310°.

[0026] Preferably, the dyeing process includes two production lines, one of which is a sheet dyeing process and the other is a rope dyeing process. The steps of the sheet dyeing process include: 1. Warping: Concentrate the cheese yarn in a sheet on an axis according to the requirements of the weaving process, in preparation for the next process of production, namely dyeing and sizing. 2. Dyeing and sizing; unwinding of the warp beam - pre-wetting (scouring) treatment 1 to 2 tanks - dyeing (padding oxidation) 6 to 12 tanks - washing 2 to 3 tanks - pre-drying - sizing - drying - skeining - reel (weaving beam). The steps of the rope dyeing process include: 1. Bunch warping: Concentrate the cheese yarn in a bundle on an axis according to the requirements of the weaving process, in preparation for the next process of production, namely dyeing; 2. Rope dyeing machine (bundle dyeing machine): Deeply dye the bundled yarn; 3. Yarn separation process: Divide the dyed yarn into sheets and wind them onto the warp beam; 4. Yarn sizing process: Sizing the yarn and rolling it into a weaving beam for weaving.

[0027] Table warp B1 sizing steps: Step 1, clean, clean the warp frame blue hair; clean the slurry tank guide roller and the slurry pressure roller; clean the drying cylinder, and wipe the skein rod. Replace the buckle teeth, clean the blue and oil mud on the yarn support roller and the rotor. Step 2, adjust the tension: warp frame tension. 2.5-3kg; inlet slurry tank tension: 20.529CN; outlet slurry tank tension: 24.1CN; dry zone tension: 900-1000MPa; winding tension:

[0028] 2.2-2.5kg; yarn support roller tension 2.2-2.5kg. Step 3, change the route: remove 4 drying cylinders (combine drying cylinders). Step 4, hanging shafts: 8 warp shafts, check shaft cards, grind shaft disc burrs, tie yarn joints, enlarge twist, tie large twist, and place layered twisted wires. Starting from the last shaft below, stick double-sided twist tape paper (find the middle line as a mark) and so on. Stick double-sided tape paper (fix the position of each line). Step 5, flower arrangement: wind yarn on the empty shaft on the head of the car. Wear the first twist tape paper at the bottom of the layered twist rod, and stop after reaching the root of the buckle tooth. Put on the buckle tooth, start from the middle marked one and arrange the buckles on both sides, put 1 yarn in each buckle tooth, and after the second twist tape paper, arrange the buckles from both sides. And so on. Step 6, slurry adjustment: when there are 3 layers left, start slurry adjustment; the slurry adjustment process includes: ① add 300 liters of water; ② raise the temperature to 70 degrees; ③ add JA-20 slurry. 4 barrels (200 liters) measure the solid content; ④ set the volume to about 600 liters. Measure the solid content to 8.3%; ⑤ put it into the slurry tank, measure the solid content to 8% and raise the temperature by 50-58 degrees. Step 7, start the machine, exit the slurry tank, the temperature of the first group of drying cylinders is 125 degrees; the temperature of the second group of drying cylinders is 110 degrees; the temperature of the combined drying cylinders is 90 degrees; the moisture regain is 5%; the speed is 60-70 meters / minute.

[0029] After the grey cloth is woven, a detection system is set up to detect defects on the grey cloth. The detection system includes an image acquisition system, a lighting system, an actuator, and a transmission system. The transmission system includes a tension roller driven by a motor, which mainly provides a stable running speed for the fabric. Too fast speed will lead to a decrease in accuracy, and too slow speed will lead to low efficiency. The speed should be selected according to the overall performance of the system. The transmission system also needs to maintain a certain tension on the surface of the fabric during operation, flattening the surface of the fabric so that the defects are fully exposed; the lighting system provides a stable and reliable light source, using multiple linear light sources for lighting, so that the light source effect is good and the control is relatively easy. Since the grey cloth is wide, with a width of more than 1.6 meters, at least 4 independent light sources are required, otherwise there will be a serious uneven lighting phenomenon, which will affect the experimental results. You can also choose to place a layer of black cloth under the cloth to increase the contrast, which will help identify some directional defects; the image acquisition system high-speed camera can take multiple photos per second, and can also use multiple cameras to work simultaneously. The DALSAHM 1024 camera is selected as the hardware for image acquisition. The maximum resolution of the camera is 1 024pixel×768pixel, and the maximum frame rate is 117 frames / s. The camera is connected to an industrial computer, and the image obtained by the camera is processed in the industrial computer; the actuator is a marking machine. If a defect is detected, it can not only be accurately displayed on the computer screen, but also use the marking machine to make detailed marks on the surface of the cloth to facilitate the smooth progress of subsequent scoring, maintenance and other operations.

[0030] After image acquisition, the image is preprocessed, and the processing steps are: 1. Image acquisition; 2. Image segmentation; 3. Image grayscale; 4. Removal of uneven illumination; 5. Image filtering; 6. Equalization; The process of image filtering is: a. Get the initial address, width and height of the original image; b. Open a buffer to temporarily store the image and initialize it; c. Scan the pixels one by one, arrange the neighborhood elements from large to small, and assign the middle value to the target point; d. Repeat the previous step until all pixels are processed; e. Extract the results in the buffer; After median filtering, the image noise is significantly suppressed and the grayscale distribution is more stable.

[0031] The method of the technical solution is used to weave a unique left twill of the surface warp yarn B1. If the thread is broken or the harness is wrong, the left twill will be defective and uneven, affecting the normal use of the grey cloth. Therefore, after obtaining image information through the camera, the left twill of the surface warp yarn B1 is detected, and the machine is stopped and adjusted in time when defects occur, so as to reduce the loss of raw materials in the manufacturing process; during the detection, when the weft yarn is perpendicular to the plane, the inclination angle of the warp yarn is within the range of -45°-+45°; the specific detection steps include: the first step is to cut the denim fabric image to obtain an image S1 with a resolution of 300 pixels × 300 pixels; the second step is to use Fourier transform on the image S1 to obtain a Fourier transform amplitude map, and the weft skew angle θ is obtained through the coordinates of the second two points. 1 ; The third step is to use directional neighborhood filtering on the transmission image and set the filter angle value to θ 1 , L value is at least 55 pixels, and image S2 with only weft information is obtained; fourth step, image S2 is subjected to image thinning processing to obtain image S3 with only weft yarn information of denim fabric; fifth step, Δρ=1, Δθ=0.1°, and (θ 1 +1°)~(θ 1 -1°), perform spatial transformation on image S3 to obtain the A(ρ, θ) matrix, measure 5 peak points, average them, and obtain the precise latitude and inclination angle θ. 2 ; The spatial transformation of image S3 is to transform a point on the original image, whose coordinates are (x, y), into a sine curve according to the following formula: ρ = xcosθ + ysinθ. In the formula: ρ is the distance from a point on the line to the origin; θ is the perpendicular line from the origin to the line. Each sine curve in the sine curve represents a point passing through a specific point (x i ,y i) The intersection points correspond to the lines passing through (x i ,y i) and (x j ,y j) Use high-resolution spatial transformation within the adjacent range of longitude and latitude angles to achieve the required precise latitude and latitude angles; improve detection accuracy.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The invention discloses a preparation process and method of a double-layer composite burnt-out denim fabric. The warp yarn has good elasticity and good wear resistance through warp drawing and sizing. The double-layer structure makes the fabric thick and dimensionally stable. After a subsequent burnt-out treatment, a pattern is formed on the surface of the denim fabric. The bottom nylon fabric not only increases the firmness and durability of the pattern, but also prevents irreversible deformation around the pattern, and significantly improves the wear resistance and washability. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 It is a product organization diagram of the present invention.

[0036] Figure 2 This is a schematic diagram of the effect of the burnt flower product of the present invention Figure 1 .

[0037] Figure 3 This is a schematic diagram of the effect of the burnt flower product of the present invention Figure 2 . DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] In addition, in the present invention, descriptions such as "first" and "second" are only used for descriptive purposes, and do not specifically refer to the order or sequence, nor are they used to limit the present invention. They are only used to distinguish components or operations described with the same technical terms, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions and technical features between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0041] Embodiment 1:

[0042] refer to Figure 1-3 A preparation process of a double-layer composite burnt-out denim fabric, a preparation process of a double-layer composite burnt-out denim fabric, characterized in that it comprises the following steps: dyeing, weaving, and post-processing; the surface warp yarn B1 is warped (warp arrangement), dyed, sizing, dried, and drawn into the weft, and then woven with the inner warp yarn A1, the surface weft yarn B2, and the inner weft yarn A2 on the machine, and then subjected to post-processing to obtain a finished fabric, and the finished fabric is subjected to a burnt-out process to form holes;

[0043] During the warp arrangement process, the outer warp yarn B1 and the inner warp yarn A1 are longitudinally arranged and wound on two warp beams, the warp beam of the inner warp yarn A1 is the sky beam, and the warp beam of the outer warp yarn B1 is the ground beam. The outer warp yarn B1 arranged on the ground beam is dyed, and the inner warp yarn A1 arranged on the sky beam is not dyed. The warp let-off ratio of the inner warp yarn A1: the outer warp yarn B1 is 2:1; the outer weft yarn A2 and the inner weft yarn B2 are not dyed, and the warp let-off ratio of the outer weft yarn A2: the inner weft yarn B2 is 2:1. The ratio is 1:2; the warp drawing adopts 12-page heald frame, among which the 2nd, 3rd, 5th, 6th, 8th, 9th, 11th and 12th pages are drawn through the inner warp yarn A1 on the sky axis, and the 1st, 4th, 7th and 10th pages are drawn through the surface warp yarn B1 on the ground axis; the side structure is 1 and 2 pages, and the ground structure is 3, 4, 5, 6, 7, 8, 9, 10, 11 and 12 pages, and the ground structure is reversed; the heald drawing method adopts the weaving method of composite structure + combined structure: 1 up and 1 down + 2 up and 1 down.

[0044] The inner warp yarn A1 and the inner weft yarn B2 are made of nylon yarn; the outer warp yarn B1 and the outer weft yarn A2 are made of flat yarn. During the warping process, the total number of warp yarns of the inner warp yarn A1 is 4339; the total number of warp yarns of the outer warp yarn B1 is 3380, and the total warp weight is 7719; the axis distance of the warp beam is 190cm. The length of the outer weft yarn A2 accounts for 33.33% of the total weft yarn length, and the yarn consumption per kilometer of the grey cloth is 134.95kg; the length of the inner weft yarn B2 accounts for 66.67% of the total weft yarn length, and the yarn consumption per kilometer of the grey cloth is 30.89kg. The reed number in the weft drawing process is 91#, the reed width is 185.7cm, and the number of yarns for the side tissue is 40+40; the number of warp threads of the ground tissue is 3, and the number of warp threads of the side tissue is 2; the weft density on the machine is 105.

[0045] In the dyeing process of warp yarn B1, the plain yarn is used as the raw material and firstly subjected to a refining treatment. The refining agent is alkyl alcohol polyoxyethylene ether fatty acid ester as the main component, the concentration is 4.5-5.5g / L, the refining temperature is 75℃, and the refining treatment is one time; after the yarn is subjected to the refining treatment, it is subjected to three water washings and water spraying to remove the residual refining agent on the yarn, and then the yarn is subjected to the dyeing treatment by the dyeing machine, and the speed of the dyeing machine is 21m / min; the dyeing temperature is 25-28℃, and the dye liquor contains Indigo, caustic soda, and insurance powder, the weight ratio of indigo: caustic soda: insurance powder is 1:1:1.2, and the concentration of caustic soda is 100-150g / L; indigo is aqueous indigo fuel, the concentration is 80-110g / L; insurance powder is sodium dithionite, the concentration is 1.5-2.5g / L; during the dyeing process, 50g / L of the above ingredients are added, and the concentration of the additional dye solution is 1.5g / L. After dyeing, the fabric is washed with water at a temperature of 50-70℃, washed three times, and the washing time is 30-40min. During the dyeing process, a biological softener is added, containing silk protein essence, the concentration is 2.5-3.5g / L, and the softening treatment temperature is 50℃.

[0046] Post-processing includes singeing, desizing, washing, pre-shrinking and drying; singeing on both sides at a speed of 110m / min, desizing using desizing enzyme at a concentration of 1g / L and penetrant at a concentration of 1g / L, desizing temperature of 60℃, and desizing vehicle speed of 55m / min; eight-tank desizing with a water temperature of 55-65℃; pre-shrinking temperature of 135-150℃, warp and weft shrinkage of 1%-4%, and the warp density of the finished grey cloth is 172 and the weft density is 120.

[0047] When the finished fabric is burnt, the acid is dissolved in the paste and sprayed on the grey cloth to form the required pattern, and then the grey cloth is baked at a high temperature of 120-130°C for 2-3 minutes and steamed at 95-97°C for 3-5 minutes; the surface warp yarn B1 and the surface weft yarn B2 at the spraying location are made of pure cotton, the water is evaporated, the acid concentration increases, the surface warp yarn B1 and the surface weft yarn B2 fibers are carbonized to become hydrated fibers with low polymerization degree and hydrolyzed to form a hole pattern; the inner warp yarn A1 and the inner weft yarn A2 are made of nylon and will not be carbonized, and a nylon mesh structure is formed at the bottom of the hole pattern.

[0048] The acid is dilute sulfuric acid with a concentration of 4.5%-6%; the paste is a mixed paste including white dextrin and dragon glue:

[0049] Emulsified paste, weight ratio is 1:1:1, concentration is 60% - 70%.

[0050] The pre-shrinking process of grey cloth adopts the short machine double shrinking method. The grey cloth passes through two sets of rubber blankets and is not connected to the mercerizing machine before pre-shrinking.

[0051] The inner warp yarn A1 and the inner weft yarn A2 use nylon line model Jinliyuan-N50+20D-non-Lycra 2.5 times, with a total warp of 4339 strands and a line type of JY1083-20T; the surface warp yarn B1 uses flat yarn model Xinyize-C9, and the surface warp yarn B2 uses flat yarn model Tianhong-C12.

[0052] The warp yarn is wrapped in the warping process, and the yarn is fixed by winding and drawn. Because nylon yarn is thin, it is drawn by small tension. The dynamic tension of the warping creel is 25-30CN, the pressure of the pressure roller is 100-200N, and the warping speed is 400-450r / min, so as to achieve the purpose of yarn flatness. In the warping process, the warp setting is simultaneously untwisted with the adjacent yarn. In the dyeing process, chemical additives are reduced, and biological additives that do not damage the yarn are used to achieve the dyeing effect.

[0053] The loom parameters used are: heald frame height 123mm; opening: 26°; back beam height 4cm; back beam depth: 4cm; warp stop frame height: -8cm; warp stop depth: 8cm; machine speed 400-450m / min; palm flat: 308-310°.

[0054] The dyeing process adopts the flake dyeing process, and the flake dyeing process steps include: 1. Warping: Concentrate the cheese yarn in a sheet on an axis according to the weaving process requirements to prepare for the next production process, namely dyeing and sizing. 2. Dyeing and sizing; warp beam unwinding - pre-wetting (scouring) treatment 1 to 2 tanks - dyeing (padding oxidation) 6 to 12 tanks - washing 2 to 3 tanks - pre-drying - sizing - drying - hank - reel (weaving shaft).

[0055] Table warp B1 sizing steps: Step 1, clean, clean the warp frame blue hair; clean the slurry tank guide roller and the slurry pressure roller; clean the drying cylinder, and wipe the skein rod. Replace the buckle teeth, clean the blue and oil mud on the yarn support roller and the rotor. Step 2, adjust the tension: warp frame tension. 2.5-3kg; inlet slurry tank tension: 20.529CN; outlet slurry tank tension: 24.1CN; dry zone tension: 900-1000MPa; winding tension:

[0056] 2.2-2.5kg; yarn support roller tension 2.2-2.5kg. Step 3, change the route: remove 4 drying cylinders (combine drying cylinders). Step 4, hanging shafts: 8 warp shafts, check shaft cards, grind shaft disc burrs, tie yarn joints, enlarge twist, tie large twist, and place layered twisted wires. Starting from the last shaft below, stick double-sided twist tape paper (find the middle line as a mark) and so on. Stick double-sided tape paper (fix the position of each line). Step 5, flower arrangement: wind yarn on the empty shaft on the head of the car. Wear the first twist tape paper at the bottom of the layered twist rod, and stop after reaching the root of the buckle tooth. Put on the buckle tooth, start from the middle marked one and arrange the buckles on both sides, put 1 yarn in each buckle tooth, and after the second twist tape paper, arrange the buckles from both sides. And so on. Step 6, slurry adjustment: when there are 3 layers left, start slurry adjustment; the slurry adjustment process includes: ① add 300 liters of water; ② raise the temperature to 70 degrees; ③ add JA-20 slurry. 4 barrels (200 liters) measure the solid content; ④ set the volume to about 600 liters. Measure the solid content to 8.3%; ⑤ put it into the slurry tank, measure the solid content to 8% and raise the temperature by 50-58 degrees. Step 7, start the machine, exit the slurry tank, the temperature of the first group of drying cylinders is 125 degrees; the temperature of the second group of drying cylinders is 110 degrees; the temperature of the combined drying cylinders is 90 degrees; the moisture regain is 5%; the speed is 60-70 meters / minute.

[0057] Embodiment 2:

[0058] On the basis of Example 1, the inner warp yarn A1 and the inner weft yarn A2 are made of nylon line model Jinliyuan-N50+30D-non-Lycra 2.5 times, the inner warp yarn A1 is used in an amount of 3700 yarns, and the line type is GY977-5TA.

[0059] Embodiment three:

[0060] On the basis of Example 1, the inner warp yarn A1 and the inner weft yarn A2 are made of nylon line model Yuexin-T75+20D-Lycra 3.0 times empty bag, the inner warp yarn A1 is used in an amount of 3700 yarns, and the line type is XR993-12TC.

[0061] Embodiment 4:

[0062] The dyeing process adopts the rope dyeing process, and the steps of the rope dyeing process include: 1. Bundle warping: according to the weaving process requirements, the cheese yarn is concentrated on an axis in a bundle to prepare for the next process, namely dyeing; 2. Rope dyeing machine (bundle dyeing machine): deep dyeing the bundled yarn; 3. Yarn separation process: divide the dyed yarn into sheets and wind them onto the warp beam; 4. Sizing process: sizing the yarn and rolling it into a weaving beam for weaving.

[0063] Embodiment five:

[0064] On the basis of Example 1, after the grey cloth is woven, a detection system is provided to detect defects on the grey cloth. The detection system includes an image acquisition system, a lighting system, an actuator, and a transmission system; the transmission system includes a tension roller driven by a motor, which mainly provides a stable running speed for the textile. Too fast speed will lead to a decrease in accuracy, and too slow speed will lead to low efficiency. The speed should be selected according to the overall performance of the system. The transmission system also needs to maintain a certain tension on the surface of the textile during operation, flatten the surface of the textile, so that the defects are fully exposed; the lighting system provides a stable and reliable light source, and uses multiple linear light sources for lighting, so that the light source effect is good and the control is relatively easy. Since the grey cloth is wide, with a width of more than one meter, at least 4 independent light sources are required, otherwise a relatively serious uneven illumination phenomenon will occur, which will affect the experimental results. You can also choose to place a layer of black cloth under the cloth to increase the contrast, which will help identify some directional defects; the image acquisition system high-speed camera can take multiple photos per second, and can also use multiple cameras to work simultaneously. The DALSAHM 1024 camera is selected as the hardware for image acquisition. The maximum resolution of the camera is 1 024pixel×768pixel, and the maximum frame rate is 117 frames / s. The camera is connected to an industrial computer, and the image obtained by the camera is processed in the industrial computer; the actuator is a marking machine. If a defect is detected, it can not only be accurately displayed on the computer screen, but also use the marking machine to make detailed marks on the surface of the cloth to facilitate the smooth progress of subsequent scoring, maintenance and other operations.

[0065] After image acquisition, the image is preprocessed, and the processing steps are: 1. Image acquisition; 2. Image segmentation; 3. Image grayscale; 4. Removal of uneven illumination; 5. Image filtering; 6. Equalization; The process of image filtering is: a. Get the initial address, width and height of the original image; b. Open a buffer to temporarily store the image and initialize it; c. Scan the pixels one by one, arrange the neighborhood elements from large to small, and assign the middle value to the target point; d. Repeat the previous step until all pixels are processed; e. Extract the results in the buffer; After median filtering, the image noise is significantly suppressed and the grayscale distribution is more stable.

[0066] The method of the technical solution is used to weave a unique left twill of the surface warp yarn B1. If the thread is broken or the harness is wrong, the left twill will be defective and uneven, affecting the normal use of the grey cloth. Therefore, after obtaining image information through the camera, the left twill of the surface warp yarn B1 is detected, and the machine is stopped and adjusted in time when defects occur, so as to reduce the loss of raw materials in the manufacturing process; during the detection, when the weft yarn is perpendicular to the plane, the inclination angle of the warp yarn is within the range of -45°-+45°; the specific detection steps include: the first step is to cut the denim fabric image to obtain an image S1 with a resolution of 300 pixels × 300 pixels; the second step is to use Fourier transform on the image S1 to obtain a Fourier transform amplitude map, and the weft skew angle θ is obtained through the coordinates of the second two points. 1 ; The third step is to use directional neighborhood filtering on the transmission image and set the filter angle value to θ 1 , L value is at least 55 pixels, and image S2 with only weft information is obtained; fourth step, image S2 is subjected to image thinning processing to obtain image S3 with only weft yarn information of denim fabric; fifth step, Δρ=1, Δθ=0.1°, and (θ 1 +1°)~(θ 1 -1°), perform spatial transformation on image S3 to obtain the A(ρ, θ) matrix, measure 5 peak points, average them, and obtain the precise latitude and inclination angle θ. 2 ; The spatial transformation of image S3 is to transform a point on the original image, whose coordinates are (x, y), into a sine curve according to the following formula: ρ = xcosθ + ysinθ. In the formula: ρ is the distance from a point on the line to the origin; θ is the perpendicular line from the origin to the line. Each sine curve in the sine curve represents a point passing through a specific point (x i ,y i) The intersection points correspond to the lines passing through (x i ,y i) and (x j ,y j) Use high-resolution spatial transformation within the adjacent range of longitude and latitude angles to achieve the required precise latitude and latitude angles; improve detection accuracy.

[0067] During the detection process, in addition to the above-mentioned warp defects, there are many kinds of defects in the cloth, and the size and shape of the defects are randomly combined and changed. Therefore, it is necessary to detect the defects without manual intervention (setting the angle and radius). By extracting the features of the image, each filter channel will generate a corresponding image, and finally a set of filtered images will be obtained; such results are often not convenient for subsequent analysis and processing due to information redundancy and lack of emphasis. It is also necessary to fuse the results of each channel. First, analyze the fusion information of each scale and select several channels for information fusion. After the first fusion is completed, select several channels with the most concentrated energy. The specific fusion steps are as follows: (1) For each channel Cq, divide the image into K non-overlapping regions, each region is L*L in size; the average output of region k in each channel satisfies: Where: k = 1, 2, K; q = 1, 2, L; (2) For the entire fused image Cq (x, y), calculate the mean μ and variance σ of the image;

[0068] μ=1 / (H·W)∑ (x,t) C q (x,y);

[0069] σ=(1 / (H·W)(x,y)-μ) 2 ) 1 / 2 ; In the above formula, H is the height of the image and W is the width of the image; (3) According to the formula in step (1), the average output is obtained and the region k is divided into an energy concentration region and an energy divergence region, represented by 1 and 0; (4) For each channel, count the number of energy concentration areas Mq, (5) Select several candidate channels q1 from step (4) and perform data fusion. The fusion result G(x, y) satisfies: G(x, y) = ∑ q1 C q1 ; According to the above process, the data information features of the image are obtained, and the extracted features are further subjected to threshold processing, opening and closing operations, and three quantities of defect features are extracted: circularity, area and perimeter. According to the common defect values, the spot stain has the smallest area and is nearly circular, so the circularity is the largest. Compared with the spot stain, the hole causes a change in the texture of the cloth, so the area increases and the circularity decreases. The horizontal fold has the lowest circularity because it is relatively slender. The oil stain has the largest area, but the shape is very irregular, so the circularity range is relatively large. The defects are classified according to the circularity, area and perimeter judged by the image, and marked by a marking machine to achieve the classification of the defects of the grey cloth, which is convenient for the subsequent further processing of the defects.

[0070] Other technical solutions not described in detail in the present invention are all existing technologies in the field and will not be described in detail here.

[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A preparation process of a double-layer composite burnt-out denim fabric, characterized in that: The following steps are involved: Dyeing, weaving, and finishing; After warping, dyeing, sizing, drying and drawing, the outer warp yarn B1 is woven with the inner warp yarn A1, the outer weft yarn B2 and the inner weft yarn A2, and then the finished cloth is processed to form a finished cloth, and the finished cloth is burnt out to form holes; During the warping process, the surface warp yarn B1 and the inner warp yarn A1 are longitudinally arranged and wound on two warp beams, the warp beam of the inner warp yarn A1 is the sky beam, and the warp beam of the surface warp yarn B1 is the ground beam. The surface warp yarn B1 arranged on the ground beam is dyed, and the inner warp yarn A1 arranged on the sky beam is not dyed. The warp let-off ratio of the inner warp yarn A1: the surface warp yarn B1 is 2:

1. The outer weft yarn A2 and the inner weft yarn B2 are not dyed, and the warp ratio of the outer weft yarn A2: the inner weft yarn B2 is 1:2; The warping process uses 12 heald frames, of which the 2nd, 3rd, 5th, 6th, 8th, 9th, 11th, and 12th pages are threaded with the inner warp yarn A1 on the sky axis, and the 1st, 4th, 7th, and 10th pages are threaded with the surface warp yarn B1 on the ground axis. The side weave is 1st and 2nd pages, and the ground weave is 3rd, 4th, 5th, 6th, 7th, 8th, 9th, 10th, 11th, and 12th pages, and the ground weave is reversely threaded; The heald lifting method adopts the weaving method of composite structure + combined structure: 1 up and 1 down + 2 up and 1 down.

2. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: The inner warp yarn A1 and the inner weft yarn B2 are made of nylon yarn; the outer warp yarn B1 and the outer weft yarn A2 are made of plain yarn.

3. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: The wheelbase of the warp beam is 190cm.

4. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: The length of the outer weft yarn A2 accounts for 33.33% of the total weft yarn length, and the yarn consumption per kilometer of the grey cloth is 134.95 kg. The length of the inner weft yarn B2 accounts for 66.67% of the total weft yarn length, and the yarn consumption per kilometer of the grey cloth is 30.89 kg.

5. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: The reed number during the drawing-in process is 91#, the reed width is 185.7cm, the number of yarns used for the edge structure is 40+40; the number of warp threads of the ground structure entering the reed is 3, and the number of warp threads of the edge structure entering the reed is 2; the weft density on the machine is 105.

6. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: In the dyeing process of warp yarn B1, the plain yarn is used as the raw material and firstly subjected to a refining treatment. The refining agent is alkyl alcohol polyoxyethylene ether fatty acid ester as the main component, the concentration is 4.5-5.5g / L, the refining temperature is 75℃, and the refining treatment is one time; after the yarn is subjected to the refining treatment, it is subjected to three water washings and water spraying to remove the residual refining agent on the yarn, and then the yarn is subjected to the dyeing treatment by the dyeing machine, and the speed of the dyeing machine is 21m / min; the dyeing temperature is 25-28℃, and the dyeing liquid contains indigo. Indigo, caustic soda, and insurance powder, the weight ratio of indigo: caustic soda: insurance powder is 1:1:1.2, and the concentration of caustic soda is 100-150g / L; indigo is aqueous indigo fuel, and the concentration is 80-110g / L; the insurance powder is sodium dithionite, and the concentration is 1.5-2.5g / L; 50g / L of the above ingredients are added during the dyeing process, and the concentration of the additional dye solution is 1.5g / L. After dyeing, the fabric is washed with water at a water temperature of 50-70℃, and washed three times for 30-40min.

7. The preparation process of a double-layer composite burnt-out denim fabric according to claim 6, characterized in that: During the dyeing process, a biological softener containing silk protein essence is added with a concentration of 2.5-3.5g / L, and the softening treatment temperature is 50°C.

8. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: Post-processing includes singeing, desizing, washing, drying and pre-shrinking; singeing on both sides at a speed of 110m / min, desizing using desizing enzyme at a concentration of 1g / L and penetrant at a concentration of 1g / L, desizing temperature of 60℃ and desizing vehicle speed of 55m / min; eight-tank desizing at a water temperature of 55-65℃; pre-shrinking temperature of 135-150℃, warp and weft shrinkage of 1%-4%, and the warp density of the finished grey cloth is 172 and the weft density is 120.

9. The preparation process of a double-layer composite burnt-out denim fabric according to claim 1, characterized in that: When the finished fabric is burnt, the acid is dissolved in the paste and sprayed on the grey cloth to form the required pattern. Then the finished fabric is baked at a high temperature of 120-130°C for 2-3 minutes and steamed at 95-97°C for 3-5 minutes. The surface warp yarn B1 and the surface weft yarn B2 at the spraying location are made of pure cotton, the water is evaporated, the acid concentration increases, the surface warp yarn B1 and the surface weft yarn B2 fibers are carbonized to become hydrated fibers with low polymerization degree and hydrolyzed to form a hole pattern. The inner warp yarn A1 and the inner weft yarn A2 are made of nylon and will not be carbonized, and a nylon mesh structure is formed at the bottom of the hole pattern.

10. The preparation process of the double-layer composite burnt-out denim fabric according to claim 9, characterized in that: The acid is dilute sulfuric acid with a concentration of 4.5%-6%; the paste is a mixed paste including white dextrin, dragon glue: emulsified paste with a weight ratio of 1:1:1 and a concentration of 60%-70%.

Citation Information

Patent Citations

  • Method for processing burnt-out revealed denim style effect denim

    CN104060488A

  • Burnt-out polar fleece fabric and production method thereof

    CN104652028A

  • Carving printing method of polyester-cotton interwoven double-layer fabric

    CN110295430A

  • Double-layer jacquard fabric and preparation process thereof

    CN116288857A

  • Denim fabric with compact structure, softness and skin friendliness

    CN216193055U

Cited By

  • Denim fabric and processing method thereof

    CN122728010A

  • Known denim fabric

    CN224799062U