Ultrafine high-elastic fiber fabric and production process thereof

Through the electrospinning of succinic anhydride modified keratin and polyamide fibers and the treatment of low-concentration sulfuric acid, the separation of silk fibers and polyamide fibers is solved, which improves the mechanical properties and stability of the fibers and reduces static electricity. risk, achieving better fiber binding and biocompatibility.

CN118727237BActive Publication Date: 2024-11-19SICHUAN TINGMANYI TECH GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411217515.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Silk fibers and polyamide fiber core yarns are prone to separation after long-term use, resulting in product quality problems. The existing adhesives may affect the spinning process and performance, increasing the risk of skin irritation.

Method used

Electrospinning with succinic anhydride acylation modified keratin and polyamide fibers are used to form disulfide bonds between proteins instead of adhesives, improving the mechanical properties and stability of the fibers, and treating the fibers with low concentration of sulfuric acid solution to enhance the The adhesion of the yarn.

Benefits of technology

It improves the mechanical properties, thermal stability and durability of the fiber, enhances the mechanical properties and interface strength of the yarn, reduces the risk of electrostatic attraction and electrostatic discharge, and improves the structural uniformity and biocompatibility of the fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KW5UPSDPBRAES4BGHBMVPC76L00CKXVGAPTHIHNR
    Figure KW5UPSDPBRAES4BGHBMVPC76L00CKXVGAPTHIHNR
  • Figure VHOQDJ4DZPM9WHH7O0UT0E6VIRXGNZKZLET49VUU
    Figure VHOQDJ4DZPM9WHH7O0UT0E6VIRXGNZKZLET49VUU
Patent Text Reader

Abstract

The invention relates to an ultra-fine high-elastic fiber fabric and a production process thereof, belonging to the technical field of fabric weaving. The ultra-fine high-elastic fiber fabric is obtained by weaving a core-spun yarn fiber prepared by using unwrapped silk fiber and modified polyamide fiber as core wire. In the process, keratin is modified by using succinic anhydride, and then used to strengthen polyamide, and the modified polyamide fiber is obtained by electrospinning, so as to improve its mechanical properties as a core wire. The covering wire and the core wire are treated with a reducing agent and a low-concentration sulfuric acid solution, and the use of an adhesive is replaced by the form of re-forming disulfide bonds between proteins, thereby improving the stability of the core-spun yarn, and the woven fiber has good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabric weaving, in particular to an ultra-fine high-elastic fiber fabric and a production process thereof. Background Art

[0002] Silk fiber is a fiber raw material with a soft and elastic feel, a smooth and uniform surface, and good tensile properties and biocompatibility. However, the diameter of silk fiber is very thin, and its toughness is not as good as other fibers, so it is prone to tearing and abrasion. Polyamide fiber, also known as nylon or nylon, is an important synthetic fiber with high tensile strength and good elastic recovery rate, and excellent wear resistance, which makes it provide excellent strength and wear resistance when used as the core yarn of core-spun yarn. The light resistance of polyamide fiber is slightly poor. It is easy to turn yellow and its strength will decrease when exposed to sunlight or ultraviolet light for a long time. The surface of polyamide fiber is smooth and waxy, which affects its feel to a certain extent.

[0003] The use of silk fiber and polyamide fiber to prepare core-spun yarn can combine the advantages of both. The high strength, wear resistance and elasticity of polyamide fiber combined with the natural environmental protection, gloss and softness of silk fiber can make the core-spun yarn have good softness and gloss while maintaining strength, and a high-quality high-elastic fiber fabric can be prepared. However, due to the characteristics of mulberry silk such as easy yarn drawing and deformation, the adhesion between mulberry silk and polyamide fiber filaments in the core-spun yarn structure is not good. After long-term use, the mulberry silk fiber and polyamide fiber filament will separate, causing product quality problems. Higher requirements are placed on the production process of core-spun yarn. If the process is not appropriate, the outer yarn may be damaged or deformed, affecting the quality and appearance of the product.

[0004] In addition, in order to improve the stability of the core yarn fiber, adhesives are sometimes used between the cover yarn and the core yarn. However, some adhesives can affect the spinning process and performance, and also increase the possibility of allergic reactions and irritation to the skin. Summary of the invention

[0005] The purpose of the present invention is to provide an ultra-fine high-elastic fiber fabric and a production process thereof to solve the problems raised in the background technology. The core-spun yarn fiber prepared by using silk fiber as the sheath and modified polyamide fiber as the core is woven to obtain an ultra-fine high-elastic fiber fabric. In the process, keratin is modified by using succinic anhydride, and then used to strengthen polyamide, and the modified polyamide fiber is obtained by electrospinning to improve its mechanical properties as the core wire. The sheath and the core wire are treated with a reducing agent and a low-concentration sulfuric acid solution, and the use of the adhesive is replaced by the re-formation of disulfide bonds between proteins, thereby improving the stability of the core-spun yarn, and the woven fiber has good mechanical properties.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0008] S1, preparing modified polyamide fiber and selecting silk fiber;

[0009] S2, pre-treating the modified polyamide fiber in step S1 to obtain a core wire; pre-treating the silk fiber to obtain a covered wire;

[0010] S3, treating the core wire and the covered wire obtained after the pretreatment using a core-spun yarn device to obtain a composite yarn;

[0011] S4, weaving the composite yarn to obtain an ultra-fine high-elastic fiber fabric;

[0012] The modified polyamide fiber is obtained by mixing keratin modified by acylation of succinic anhydride with polyamide, dissolving the mixture and then electrostatically spinning the mixture.

[0013] Further, in step S1, the modified polyamide fiber is prepared by the following steps:

[0014] A1. Cut the keratin raw material into pieces, grind and sieve, then put it into deionized water, add urea, sodium pyrosulfite and sodium dodecyl sulfate into the system, stir evenly, adjust the pH value of the system to 6-7, increase the system temperature to 60°C-70°C, and stir for 2-4 hours;

[0015] A2, centrifuging the product obtained in step A1, then discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0, then dialyzing the system using a dialysis bag to obtain a dialyzed product, freeze-drying, and obtaining modified keratin;

[0016] A3. Dissolve the modified keratin and polyamide in formic acid at a mass ratio of (0.5-2):(28-29), stir evenly, and obtain an electrospinning solution; transfer the electrospinning solution to an electrospinning machine for electrospinning, and obtain modified polyamide fibers.

[0017] Further, in step S1, the modified polyamide fiber is prepared by the following steps:

[0018] A1. Cut the keratin raw material into pieces, grind and sieve, then put it into deionized water, add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution, increase the system temperature to 60°C-70°C, and stir for 2-4 hours;

[0019] In the above reaction process, urea is used to destroy the hydrogen bonds between protein molecules, so that the protein molecules unfold, expose the internal hydrophobic groups, open the tight structure of keratin, and make it easier to be chemically treated; sodium metabisulfite is added to the system. Some amino acids in keratin (such as cystine and cysteine) contain sulfur atoms. These sulfur atoms may form disulfide bonds under oxidative conditions, making the keratin structure more stable and difficult to process. The addition of sodium metabisulfite can prevent the occurrence of this oxidation reaction, which is beneficial to the dissolution and subsequent treatment of keratin; at the same time, sodium dodecyl sulfate is used to reduce the interaction between keratin molecules.

[0020] A2, the product obtained in step A1 was centrifuged at 8000rpm for 60 minutes, the supernatant was discarded, deionized water was added, and then 5mol / L NaOH solution was used to adjust the pH value of the system to 8.0, then succinic anhydride was added to the system, and stirring was continued until uniform, 5mol / L NaOH solution was used again to adjust the pH value of the system to 8.0, and then the system was dialyzed using a dialysis bag, the dialysis bag cutoff was 14000Da, distilled water was added every 6 hours of dialysis, and the total dialysis time was 72 hours to obtain a dialysis product, which was freeze-dried to obtain modified keratin;

[0021] In the above reaction process, keratin is acylated with succinic anhydride, and an acyl group is introduced into keratin by utilizing a nucleophilic substitution reaction between the amino groups contained in the amino acids of keratin and the anhydride in succinic anhydride to obtain modified keratin.

[0022] A3. Dissolve the modified keratin and polyamide in formic acid at a mass ratio of (0.5-2):(28-29), stir evenly, and obtain an electrospinning solution; transfer the electrospinning solution to an electrospinning machine for electrospinning, and obtain modified polyamide fibers.

[0023] Furthermore, in step A1, the mass ratio of keratin raw material, urea, sodium metabisulfite and sodium dodecyl sulfate is (1-3): (45-50): (7-10): (1-2).

[0024] Furthermore, in step A3, the specific operation of the electrospinning treatment is: at room temperature, at a speed of 0.05-0.2 ml / h and a voltage of 18-22 kV, the distance between the spinning needle tip and the receiver is controlled to be 10-30 cm, and then electrospinning is performed.

[0025] Further, in step S2, the core wire is specifically prepared by the following steps:

[0026] The modified polyamide fiber obtained in step S1 is immersed in a 1-3wt% sulfuric acid solution for 5-10 hours, rinsed with deionized water, and then the water is drained to obtain a core wire.

[0027] Further, in step S2, the covered wire is specifically prepared by the following steps:

[0028] Select silk fibers, immerse the silk fibers in a mercaptoethanol solution for 5-20 minutes, then adjust the pH value of the system to 9-10, stir evenly and continue immersing for 1-2 minutes, take out and drain to obtain a wrapped wire.

[0029] Further, in step S2, the covered wire is specifically prepared by the following steps:

[0030] Select a 100NM / 2 silk fiber, immerse the silk fiber in a 10-50nmol / L mercaptoethanol solution for 5-20 minutes, then use a NaOH solution to adjust the pH of the system to 9-10, stir evenly and continue immersing for 1-2 minutes, take out and drain to obtain a wrapped wire.

[0031] Furthermore, in step S3, the specific preparation method of the composite yarn is:

[0032] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device are controlled to be 4-6kg and the speed is 100-150 m / min, and then the core yarn is stretched by the stretching device and twisted by the spinning device, wherein the stretching multiple of the stretching device is 2.5-3.5 and the stretching speed is 200-220 m / min; the twist of the spinning device is 300-500 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200-250 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn.

[0033] Furthermore, in step S4, the specific operation of spinning the composite yarn is as follows:

[0034] Composite yarn is used as warp and weft, and the warp and weft are led to the drawing-in frame at a speed of 100-200 m / min for twisting and drawing, and then the yarn is combed. The combed yarn is placed on the flannel cloth of the yarn clamping plate of the drawing-in frame, and then the clamping plate is clamped, and the weft density is set to 0.6-0.9 times the warp density; the heald frame is fixed to the drawing-in frame with a rope, and then the heald is drawn in and the reed is passed. A ruler is used to check whether there are wrong healds and wrong reed teeth on the reed. After checking, it is delivered to the loom for weaving.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) In the technical solution of the present invention, keratin acylated with succinic anhydride is mixed with a polyamide matrix, and then electrospinning is performed to prepare modified polyamide fibers. The modified keratin introduces negatively charged acyl groups, which weakens the interaction between proteins, stretches the structure of the keratin molecules, improves the crystallinity of the protein, and makes it similar to the crystallinity of polyamide. When the crystallization behaviors of the two are similar, they are more likely to form an interwoven crystalline structure when blending to prepare fibers. This crystalline structure can increase the mechanical properties, thermal stability and durability of the fiber. The two materials are more likely to be dispersed and evenly distributed in the fiber, avoiding phase separation or aggregation. This uniform dispersion helps to improve the mechanical properties and structural uniformity of the fiber. The compatibility between keratin and the polyamide matrix is ​​enhanced, which helps to improve the interface strength and durability of the core-spun yarn fiber and reduce interface peeling and fracture during processing or washing.

[0037] In addition, after acylation of keratin, the negative charge density on the surface of keratin increases, causing the isoelectric point of keratin to migrate to a lower pH, closer to the isoelectric point of polyamide, which helps to reduce phase separation, precipitation and aggregation, and is easier to form a uniform solution during the blending process. It can also reduce the electrostatic attraction and electrostatic discharge risks of the fiber during preparation and use, improve the stability of the fiber, and reduce fiber deformation, breakage or surface damage caused by static electricity. Keratin and polyamide matrices with similar isoelectric points are more likely to form a tight bond and interaction at the interface, thereby improving the interfacial strength, durability and tensile resistance of the fiber. This helps to improve the mechanical properties, thermal stability and durability of the fiber, making it more suitable for various applications.

[0038] (2) In the technical solution of the present invention, silk is used as the outer yarn, and its good air permeability, moisture permeability and comfortable, soft touch can be combined with the core yarn to optimize the structure and characteristics of the yarn. The mulberry silk-coated modified polyamide fiber uses mulberry silk as the outer yarn and the modified polyamide fiber as the core yarn. The resulting composite yarn has both the high elasticity of polyamide fiber and the good air permeability and skin-friendly properties of mulberry silk.

[0039] (3) In the technical solution of the present invention, the prepared modified polyamide fiber is subjected to a sulfuric acid roughening treatment, which can cause physical and chemical changes on the fiber surface, making its surface morphology rougher and more porous. This rough surface structure helps to increase the specific surface area of ​​the fiber, providing more active sites and adsorption capacity. For modified keratin and polyamide blended fibers, the sulfuric acid roughening treatment can further improve the surface morphology of the fiber, increase its contact area with the surrounding environment, and improve the performance in terms of adsorption, moisture absorption and biocompatibility. The introduction of modified keratin improves the hydrophilicity of the fiber, can promote the roughening effect of sulfuric acid on the modified fiber, further increase the specific surface area of ​​the fiber after roughening, and will not affect the overall mechanical properties of the fiber.

[0040] (4) In the technical solution of the present invention, mercaptoethanol is used as a reducing agent to destroy the disulfide bond structure of the fiber surface protein, so that the protein molecular chain on the fiber surface is opened, and then the surface pH value is adjusted to 9-10, and then fed into the core-spun yarn machine for processing. During the process, the exposed thiol groups on the silk fiber structure will form new disulfide bonds with keratin, thereby improving the stability between the inner and outer layers of the core-spun yarn. DETAILED DESCRIPTION

[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The keratin raw material used in the following examples and comparative examples is duck feathers, the silk fiber used is provided by Haiyan Jinyi Silk Spinning Co., Ltd. with a product number of S100100NM / 2, and the model of the polyamide used is PA66.

[0043] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0044] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0045] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 60°C and stir for 2 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1.

[0046] A2, centrifuging the product obtained in step A1 at 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then dialyzing the system with a dialysis bag, the dialysis bag cutoff is 14000Da, adding distilled water every 6 hours of dialysis, the total dialysis time is 72 hours, obtaining a dialysis product, freeze-drying, and obtaining modified keratin; wherein the mass ratio of keratin raw material to succinic anhydride is 1:0.05;

[0047] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0048] S2, soaking the modified polyamide fiber obtained in step S1 in a 1wt% sulfuric acid solution for 5 hours, washing with deionized water, and then draining the water to obtain a core wire;

[0049] The silk fiber was immersed in a 10 nmol / L mercaptoethanol solution for 5 minutes, and then the pH of the system was adjusted to 9 with a NaOH solution. After stirring evenly, the silk fiber was immersed for another minute, and then the silk fiber was taken out and drained to obtain a wrapped yarn.

[0050] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0051] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0052] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0053] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0054] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0055] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 65°C and stir for 3 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 2:48:8:1.5.

[0056] A2, centrifuging the product obtained in step A1 at a rate of 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then using 5mol / L NaOH solution to adjust the pH value of the system to 8.0, then adding succinic anhydride to the system, continuing to stir until uniform, again using 5mol / L NaOH solution to adjust the pH value of the system to 8.0, then using a dialysis bag to dialyze the system, the dialysis bag has a cutoff of 14000Da, and distilled water is added every 6 hours of dialysis, the total dialysis time is 72 hours, and a dialysis product is obtained, freeze-dried, and modified keratin is obtained; wherein the mass ratio of keratin raw material to succinic anhydride is 2:0.07;

[0057] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 1.2:28.5, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.1 ml / h and a voltage of 20 kV, controlling the distance between the spinning needle tip and the receiver to be 22 cm, to obtain modified polyamide fibers;

[0058] S2, soaking the modified polyamide fiber obtained in step S1 in a 2wt% sulfuric acid solution for 8 hours, washing with deionized water, and then draining the water to obtain a core wire;

[0059] Select silk fibers, immerse the silk fibers in a 30 nmol / L mercaptoethanol solution for 12 minutes, then adjust the pH of the system to 9 using a NaOH solution, stir evenly and continue immersing for 2 minutes, take out and drain to obtain a wrapped wire;

[0060] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0061] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 5 kg and the speed is 120 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 3 and the drafting speed is 210 m / min; the twist of the spinning device is 400 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 220 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0062] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 150 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, and you will get an ultra-fine high-elastic fiber fabric.

[0063] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0064] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0065] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 70°C and stir for 4 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 3:50:10:2.

[0066] A2, centrifuging the product obtained in step A1 at a rate of 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then using 5mol / L NaOH solution to adjust the pH value of the system to 8.0, then adding succinic anhydride to the system, continuing to stir until uniform, again using 5mol / L NaOH solution to adjust the pH value of the system to 8.0, then using a dialysis bag to dialyze the system, the dialysis bag has a cutoff of 14000Da, and distilled water is added every 6 hours of dialysis, the total dialysis time is 72 hours, and a dialysis product is obtained, freeze-dried, and modified keratin is obtained; wherein the mass ratio of keratin raw material to succinic anhydride is 3:0.08;

[0067] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 2:29, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.2 ml / h and a voltage of 22 kV, controlling the distance between the spinning needle tip and the receiver to be 30 cm, to obtain modified polyamide fibers;

[0068] S2, soaking the modified polyamide fiber obtained in step S1 in a 3wt% sulfuric acid solution for 10 hours, rinsing with deionized water, and then draining the water to obtain a core wire;

[0069] Select silk fibers, immerse the silk fibers in a 50 nmol / L mercaptoethanol solution for 20 minutes, then adjust the pH of the system to 10 using a NaOH solution, stir evenly and continue immersing for 2 minutes, take out and drain to obtain a wrapped wire;

[0070] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0071] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 6 kg and the speed is 150 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 3.5 and the drafting speed is 220 m / min; the twist of the spinning device is 500 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 250 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0072] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the drawing frame clamping plate, then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0073] Comparative Example 1

[0074] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0075] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0076] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 60°C and stir for 2 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1.

[0077] A2, centrifuging the product obtained in step A1 at 8000 rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, and then dialyzing the system using a dialysis bag with a cutoff of 14000 Da, adding distilled water every 6 hours of dialysis, and the total dialysis time is 72 hours to obtain a dialyzed product, freeze-drying, and obtaining modified keratin;

[0078] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0079] S2, soaking the modified polyamide fiber obtained in step S1 in a 1wt% sulfuric acid solution for 5 hours, washing with deionized water, and then draining the water to obtain a core wire;

[0080] Select silk fibers, immerse the silk fibers in a 10 nmol / L mercaptoethanol solution for 5 minutes, then adjust the pH of the system to 9 using a NaOH solution, stir evenly and continue immersing for 1 minute, take out and drain to obtain a wrapped wire;

[0081] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0082] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0083] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0084] Comparative Example 2

[0085] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0086] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0087] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 60°C and stir for 2 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1.

[0088] A2, centrifuging the product obtained in step A1 at 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then dialyzing the system with a dialysis bag, the dialysis bag cutoff is 14000Da, adding distilled water every 6 hours of dialysis, the total dialysis time is 72 hours, obtaining a dialysis product, freeze-drying, and obtaining modified keratin; wherein the mass ratio of keratin raw material to succinic anhydride is 1:0.05;

[0089] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0090] S2, soaking the modified polyamide fiber obtained in step S1 in a 10wt% sulfuric acid solution for 5 hours, rinsing with deionized water, and then draining the water to obtain a core wire;

[0091] Select silk fibers, immerse the silk fibers in a 10 nmol / L mercaptoethanol solution for 5 minutes, then adjust the pH of the system to 9 using a NaOH solution, stir evenly and continue immersing for 1 minute, take out and drain to obtain a wrapped wire;

[0092] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0093] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0094] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0095] Comparative Example 3

[0096] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0097] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0098] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 60°C and stir for 2 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1.

[0099] A2, centrifuging the product obtained in step A1 at 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then dialyzing the system with a dialysis bag, the dialysis bag cutoff is 14000Da, adding distilled water every 6 hours of dialysis, the total dialysis time is 72 hours, obtaining a dialysis product, freeze-drying, and obtaining modified keratin; wherein the mass ratio of keratin raw material to succinic anhydride is 1:0.05;

[0100] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0101] S2, soaking the modified polyamide fiber obtained in step S1 in deionized water for 5 hours and then draining the water to obtain a core wire;

[0102] Select silk fibers, immerse the silk fibers in a 10 nmol / L mercaptoethanol solution for 5 minutes, then adjust the pH of the system to 9 using a NaOH solution, stir evenly and continue immersing for 1 minute, take out and drain to obtain a wrapped wire;

[0103] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0104] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0105] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0106] Comparative Example 4

[0107] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0108] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0109] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 60°C and stir for 2 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1.

[0110] A2, centrifuging the product obtained in step A1 at 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then dialyzing the system with a dialysis bag, the dialysis bag cutoff is 14000Da, adding distilled water every 6 hours of dialysis, the total dialysis time is 72 hours, obtaining a dialysis product, freeze-drying, and obtaining modified keratin; wherein the mass ratio of keratin raw material to succinic anhydride is 1:0.05;

[0111] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0112] S2, soaking the modified polyamide fiber obtained in step S1 in a 1wt% sulfuric acid solution for 5 hours, washing with deionized water, and then draining the water to obtain a core wire;

[0113] Select silk fibers, immerse the silk fibers in deionized water for 10 minutes, then take them out and drain them to obtain a wrapped yarn;

[0114] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0115] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0116] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0117] Comparative Example 5

[0118] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0119] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0120] A1. Cut the keratin raw material into pieces, grind it through a 60-mesh sieve, and then put it into deionized water at a mass volume ratio of 1 g:20 mL. Add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, and adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution. Raise the system temperature to 60°C and stir for 2 hours. The mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1.

[0121] A2, centrifuging the product obtained in step A1 at a rate of 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then using 5mol / L NaOH solution to adjust the pH value of the system to 8.0, then adding acetic anhydride to the system, continuing to stir until uniform, again using 5mol / L NaOH solution to adjust the pH value of the system to 8.0, then using a dialysis bag to dialyze the system, the dialysis bag has a cutoff of 14000Da, and distilled water is added every 6 hours of dialysis, the total dialysis time is 72 hours, and a dialysis product is obtained, freeze-dried, and modified keratin is obtained; wherein the mass ratio of keratin raw material to acetic anhydride is 1:0.05;

[0122] A3, dissolving the modified keratin and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0123] S2, soaking the modified polyamide fiber obtained in step S1 in a 1wt% sulfuric acid solution for 5-10 hours, washing with deionized water, and then drying the water to obtain a core wire;

[0124] Select silk fibers, immerse the silk fibers in a 10 nmol / L mercaptoethanol solution for 5 minutes, then adjust the pH of the system to 9 using a NaOH solution, stir evenly and continue immersing for 1 minute, take out and drain to obtain a wrapped wire;

[0125] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0126] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0127] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0128] Comparative Example 6

[0129] A production process of ultra-fine high-elastic fiber fabrics, comprising the following steps:

[0130] S1. Preparing modified polyamide fiber and selecting silk fiber; wherein the modified polyamide fiber is prepared by the following steps:

[0131] A1. Add wheat protein into deionized water at a mass volume ratio of 1 g:20 mL, add urea, sodium pyrosulfite and sodium dodecyl sulfate to the system, stir evenly, adjust the pH value of the system to 6.5 with 5 mol / L NaOH solution, increase the system temperature to 60°C, and stir for 2 hours; wherein the mass ratio of keratin raw material, urea, sodium pyrosulfite and sodium dodecyl sulfate is 1:45:7:1;

[0132] A2, centrifuging the product obtained in step A1 at 8000rpm for 60 minutes, discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0 with a 5mol / L NaOH solution, then dialyzing the system with a dialysis bag, the dialysis bag cutoff is 14000Da, adding distilled water every 6 hours of dialysis, the total dialysis time is 72 hours, obtaining a dialyzed product, freeze-drying, and obtaining modified wheat protein; wherein the mass ratio of wheat protein to succinic anhydride is 1:0.05;

[0133] A3, dissolving the modified wheat protein and polyamide in formic acid at a mass ratio of 0.5:28, stirring evenly to obtain an electrospinning solution; transferring the electrospinning solution to an electrospinning machine and electrospinning at room temperature at a speed of 0.05 ml / h and a voltage of 18 kV, controlling the distance between the spinning needle tip and the receiver to be 12 cm, to obtain modified polyamide fibers;

[0134] S2, soaking the modified polyamide fiber obtained in step S1 in a 1wt% sulfuric acid solution for 5-10 hours, washing with deionized water, and then drying the water to obtain a core wire;

[0135] Select silk fibers, immerse the silk fibers in a 10 nmol / L mercaptoethanol solution for 5 minutes, then adjust the pH of the system to 9 using a NaOH solution, stir evenly and continue immersing for 1 minute, take out and drain to obtain a wrapped wire;

[0136] S3, the core wire and the covered wire obtained after the pretreatment are processed by a core-spun yarn device to obtain a composite yarn, and the specific operation is as follows:

[0137] The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device is controlled to be 4kg and the speed is 100 m / min, and then the core yarn is drafted by the drafting device and twisted by the spinning device, wherein the drafting multiple of the drafting device is 2.5 and the drafting speed is 200 m / min; the twist of the spinning device is 300 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn;

[0138] S4. Use composite yarn as warp and weft, weave a sample with plain weave structure, lead the warp and weft to the drawing frame at a speed of 100-200 m / min for twisting and twisting, then comb the yarn, place the combed yarn on the flannel of the yarn clamping plate of the drawing frame, and then clamp the clamping plate, set the weft density to 5 strands / cm, and the warp density to 4 strands / cm; use a rope to fix the heald frame to the drawing frame, then draw in and reed, with a total warp of 7080 strands, use 53.5# reed, 4 reeds, and a reed width of 66.1 inches. Use a ruler to check whether there are wrong healds and wrong reed teeth on the reed. After checking, deliver it to the loom and put it on the shaft for weaving, so as to obtain an ultra-fine high-elastic fiber fabric.

[0139] The fabrics prepared in Examples 1-3 and Comparative Examples 1-6 are now tested for mechanical properties. The weft tear strength is measured according to the trapezoidal method in GB / T 3917-2009 "Tear Properties of Textile Fabrics". The core-spun yarn fabric is tested using a tensile testing machine to test its elastic elongation and elastic recovery. Elastic elongation (%) = [(Ln-Lo) / Lo] × 100%, where Lo is the initial length and Ln is the length after stretching. Elastic recovery (%) = [(Lr-Lf) / (Lf-Lo)] × 100%, where Lf is the maximum elongation length and Lr is the length after recovery. Five readings are obtained for each sample and the average value is taken. The test results are shown in Table 1 below.

[0140] Table 1 Mechanical properties test of fabrics prepared in Examples 1-3 and Comparative Examples 1-6

[0141]

[0142] It can be seen from the results in Table 1 that the fabric prepared in Example 2 has the best mechanical properties including weft tear strength, elastic elongation and elastic recovery. It can be seen from the results in Comparative Example 1 that the modified keratin raw material is used to reinforce the polyamide fiber, which can improve the structural stability of the core yarn material, and due to the rigidity of keratin, the unmodified keratin sample significantly reduces the tensile properties of the fabric. It can be seen from the results in Comparative Examples 2 and 3 that the core wire is roughened in a sulfuric acid solution under a low concentration range to improve the bonding strength of the two fibers. It can be seen from the results in Comparative Example 4 that the bonding effect between the fabrics is reduced without using a reducing agent to treat the wire, and the mechanical properties are not significantly improved. It can be seen from the results in Comparative Examples 5 and 6 that different types of proteins have different effects after being modified by different acylating agents. Due to the difference in solubility and electronegativity with the polyamide material in the solvent, the performance improvement of the fabric is not very obvious.

[0143] Now, the fabrics prepared in Examples 1-3 and Comparative Examples 1-6 are tested for quality. The fabrics prepared in different groups are washed in 50°C water at a rate of 1200 rpm for 30 minutes, left to stand for 10 minutes, and then washed again. After repeating 10 rounds, the fabrics are tested for quality. The appearance of the core-spun yarn fabric is observed to check for displacement, shrinkage, wrinkles, surface deformation, etc. The grade standards are:

[0144] A: No wrinkles, shrinkage, deformation or displacement on the surface

[0145] B: No obvious wrinkles on the surface, shrinkage rate ≤ 98%, no obvious deformation, no obvious displacement

[0146] C: Slight wrinkles on the surface, shrinkage ≤ 95%, slight deformation, slight displacement

[0147] D: The surface has obvious wrinkles, shrinkage rate>90%, obvious deformation, and exposed core

[0148] The test results are shown in Table 2.

[0149] Table 2 Quality test of fabrics prepared in Examples 1-3 and Comparative Examples 1-6

[0150]

[0151] From the results in Table 2, it can be seen that the fabrics prepared in Examples 1-3 have the most stable quality and the core-spun yarn structure is the most stable. From the results in Comparative Examples 1-3, it can be seen that modifying the keratin raw material and roughening the core yarn with low-concentration sulfuric acid can improve the quality stability of the fabric. From the results in Comparative Example 4, it can be seen that using a reducing agent to treat the silk fiber can improve the bonding effect between the core yarn and the sheath. From the results in Comparative Examples 5 and 6, it can be seen that the modified keratin prepared by acylation treatment between succinic anhydride and keratin raw materials can improve the bonding effect between polyamide fiber and sheath, and improve the quality stability of the core-spun yarn fabric obtained.

[0152] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0153] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A production process for ultra-fine high-elastic fiber fabric, characterized in that: The following steps are involved: S1, preparing modified polyamide fiber and selecting silk fiber; S2, pre-treating the modified polyamide fiber in step S1 to obtain a core wire; pre-treating the silk fiber to obtain a covered wire; Wherein, the core wire is specifically prepared by the following steps: The modified polyamide fiber obtained in step S1 is immersed in a 1-3wt% sulfuric acid solution for 5-10 hours, then rinsed with deionized water, and then the water is drained to obtain a core wire; The covered wire is specifically prepared by the following steps: Select silk fibers, immerse the silk fibers in a mercaptoethanol solution for 5-20 minutes, then adjust the pH of the system to 9-10, stir evenly and continue immersing for 1-2 minutes, take out and drain to obtain a wrapped wire; S3, treating the core wire and the covered wire obtained after the pretreatment using a core-spun yarn device to obtain a composite yarn; S4, weaving the composite yarn to obtain an ultra-fine high-elastic fiber fabric; The modified polyamide fiber is obtained by mixing keratin modified by acylation of succinic anhydride and polyamide, dissolving and then electrostatically spinning, wherein the keratin raw material is duck feathers.

2. The production process of a superfine high elastic fiber fabric according to claim 1, characterized in that: The modified polyamide fiber is prepared by the following steps: A1. Cut the keratin raw material into pieces, grind and sieve, then put it into deionized water, add urea, sodium pyrosulfite and sodium dodecyl sulfate into the system, stir evenly, adjust the pH value of the system to 6-7, increase the system temperature to 60°C-70°C, and stir for 2-4 hours; A2, centrifuging the product obtained in step A1, then discarding the supernatant, adding deionized water to the original volume, then adjusting the pH value of the system to 8.0, then adding succinic anhydride to the system, continuing to stir until uniform, again adjusting the pH value of the system to 8.0, then dialyzing the system using a dialysis bag to obtain a dialyzed product, freeze-drying, and obtaining modified keratin; A3, dissolving the modified keratin and polyamide in formic acid in a mass ratio of (0.5-2): (28-29), stirring evenly, to obtain an electrospinning solution; The electrospinning solution is transferred to an electrospinning machine for electrospinning to obtain modified polyamide fibers.

3. The production process of a superfine high elastic fiber fabric according to claim 2, characterized in that: In step A1, the mass ratio of keratin raw material, urea, sodium metabisulfite and sodium dodecyl sulfate is (1-3):(45-50):(7-10):(1-2).

4. The production process of a superfine high elastic fiber fabric according to claim 2, characterized in that: In step A3, the specific operation of the electrospinning process is: At room temperature, at a speed of 0.05-0.2 ml / h and a voltage of 18-22 kV, the distance between the spinning needle tip and the receiver is controlled to be 10-30 cm, and then electrospinning is performed.

5. The production process of a superfine high elastic fiber fabric according to claim 1, characterized in that: In step S3, the specific preparation method of the composite yarn is: The core yarn and the covering yarn obtained in step S2 are wound on a bobbin to prepare for loading; then the core yarn and the covering yarn are respectively introduced into the core yarn feeding device and the covering yarn feeding device in the core yarn equipment, and the tension of the core yarn feeding device and the covering yarn feeding device are controlled to be 4-6kg and the speed is 100-150 m / min, and then the core yarn is stretched by the stretching device and twisted by the spinning device, wherein the stretching multiple of the stretching device is 2.5-3.5 and the stretching speed is 200-220 m / min; the twist of the spinning device is 300-500 twists / m, and then the core yarn is introduced into the winding device at a winding speed of 200-250 m / min, and the obtained core yarn is wound into a yarn tube to obtain a composite yarn.

6. The production process of a superfine high elastic fiber fabric according to claim 1, characterized in that: In step S4, the specific operation of spinning the composite yarn is as follows: Composite yarn is used as warp and weft, and the warp and weft are led to the drawing-in frame at a speed of 100-200 m / min for twisting and drawing, and then the yarn is combed. The combed yarn is placed on the flannel of the yarn clamping plate of the drawing-in frame, and then the clamping plate is clamped, and the weft density is set to 0.6-0.9 times the warp density; the heald frame is fixed to the drawing-in frame with a rope, and then the heald is drawn in and the reed is passed. A ruler is used to check whether there are wrong healds and wrong reed teeth on the reed. After the inspection is correct, it is delivered to the loom and put on the shaft for weaving.