Efficient coating process for coated white board paper

By introducing calcium carbonate particles and hollow spherical structures into the coating, combined with kaolin, to form ink absorption channels, and adjusting the position of the particles during the calendering process, the problem of low ink absorption rate of coated whiteboard paper is solved, and the printing quality and Image clarity.

CN118727504AActive Publication Date: 2024-10-01浙江金华丁丁实业有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410613430.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-01
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

The ink absorption rate of existing coated whiteboard paper is low, which affects printability and image clarity.

Method used

By introducing calcium carbonate particles and hollow spherical structures into the coating, combined with kaolin clay, ink absorption pores are formed, and the position of the particles is adjusted during the calendering process to improve the ink absorption performance of the coating.

Benefits of technology

Significantly improves ink absorption rate and printing quality, enhances the smoothness and gloss of coated whiteboard paper, and improves printability and image clarity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004844340360000021
    Figure BDA0004844340360000021
  • Figure BDA0004844340360000071
    Figure BDA0004844340360000071
  • Figure BDA0004844340360000072
    Figure BDA0004844340360000072
Patent Text Reader

Abstract

The invention discloses an efficient coating process for coated white board paper. The efficient coating process comprises the following steps: S1, coating a coating on the surface of coated paper by using a coating machine; the pigment in the coating comprises kaolin and calcium carbonate, the calcium carbonate is calcium carbonate particles generated along a chain structure of polyvinyl alcohol and calcium carbonate of a hollow spherical structure generated around sodium carboxymethyl cellulose in situ in the mixing process of the coating, and the calcium carbonate is uniformly dispersed among the kaolin particles; gaps between the flaky kaolin and the calcium carbonate particles are communicated with the hollow spherical structure of the calcium carbonate to form ink absorption pore channels; s2, drying the coated paper coated with the coating layer; s3, the dried coated white board is subjected to press polish finishing, in the press polish process, kaolin relatively shifts and slides up and down on the calcium carbonate hollow balls and / or the calcium carbonate particles, and the target coated white board is obtained; by improving the composition of the coating, the coating processing efficiency is effectively improved, and the ink absorption rate is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coated white board paper, in particular to an efficient coating process for coated white board paper. Background Art

[0002] Coated white paper is composed of a coating layer and a coated base paper. The coating layer is composed of pigments, adhesives and additives. The coating layer is used to cover the surface of the ordinary paper with unevenness and large gaps formed by the fibers on the coated base paper with a layer of coating composed of fine ions that has good ink absorption, and then a paper with good uniformity and smoothness is obtained. Coating can also improve the glossiness of the paper, improve the stability and opacity of the paper, and improve the grade of the product.

[0003] The existing coating layer is a uniform coating obtained by coating. The coating comprises a pigment, an adhesive and a dispersant, etc., wherein the adhesive bonds the pigment particles to the base paper and makes the pigment particles bond to each other.

[0004] Kaolin with a hexagonal flake structure is a commonly used pigment for coating white board paper. After the hexagonal flake kaolin is coated on the base paper, it has a high reflectivity to light, and the resulting coated white board paper has good smoothness and glossiness. However, the oil absorption value of kaolin is low, which is not conducive to the printability of coated paper. Summary of the invention

[0005] The purpose of the present invention is to provide an efficient coating process for coating white board paper. The present invention improves the coating composition, effectively improves the efficiency of the coating process, and significantly improves the ink absorption rate.

[0006] To solve this technical problem, the technical solution of the present invention is: an efficient coating process for coating white board paper, comprising the following steps:

[0007] S1, applying the coating on the surface of the coated paper using a coating machine;

[0008] The pigment in the coating includes kaolin and calcium carbonate, wherein the calcium carbonate is in-situ generated during the mixing process of the coating, and the calcium carbonate particles are generated along the polyvinyl alcohol chain structure and the hollow spherical structure calcium carbonate is generated around the sodium carboxymethyl cellulose, and the calcium carbonate is evenly dispersed between the kaolin particles; the gaps between the flaky kaolin and the calcium carbonate particles are connected with the hollow spherical structure of the calcium carbonate to form absorption channels for the ink;

[0009] S2, drying the coated paper coated with the coating layer;

[0010] S3, calendering and finishing the dried coated white board paper, during the calendering process, kaolin is relatively displaced and slid above and below the calcium carbonate hollow spheres and / or calcium carbonate particles, to obtain the target coated white board paper.

[0011] The coating composition used for the coating layer of the coated white paper preferably includes the following substances in parts by mass:

[0012]

[0013] The pigment in the present invention comprises kaolin and calcium carbonate, wherein kaolin is the main component, and the calcium carbonate generated in situ in the coating slurry is uniformly generated through a precipitation reaction, and the sodium chloride generated at the same time is used as an inorganic thickener to improve the viscosity of the obtained slurry, and the amount of calcium carbonate generated is controlled to avoid the aggregation of polyvinyl alcohol molecular chains caused by the salting-out effect due to excessive sodium chloride, thereby ensuring that the rheological properties of the coating are suitable for construction.

[0014] The preferred method for preparing the coating comprises the following steps:

[0015] S11, calcium chloride, polyvinyl alcohol, carboxymethyl cellulose, cationic color fixing agent and defoaming agent are mixed evenly according to the target mass fractions; the carboxyl group of sodium carboxymethyl cellulose and polyvinyl alcohol are mixed with Ca 2+ Chelation;

[0016] S12, adding kaolin according to the mass fraction into the slurry obtained in S11 and stirring evenly;

[0017] S13, add calcium chloride solution in an amount equal to that of sodium carbonate to the mixture in S12, stir at a constant speed, and CaCl 2 and Na 2 CO 3 Precipitation reactions occur around sodium carboxymethylcellulose and polyvinyl alcohol between kaolin particles;

[0018] S14, adding deionized water to adjust the solid content of the obtained coating to obtain the target coating.

[0019] In the process of preparing the coating slurry, the calcium ions of calcium chloride are first chelated with polyvinyl alcohol and sodium carboxymethyl cellulose respectively, and then kaolin is added, so as to effectively avoid the coagulation phenomenon between kaolin and polyvinyl alcohol during mixing, which may cause uneven coating.

[0020] Preferably, the constant speed stirring process condition in S13 is 800 r / min to 1000 r / min, and the stirring time is 45 min to 65 min;

[0021] The relatively high-speed stirring combined with the presence of kaolin particles inhibits the continuous growth of the crystal nuclei formed by the calcium carbonate around the sodium carboxymethyl cellulose and polyvinyl alcohol in the precipitation reaction or orderly stacking and assembling into large particles. The small particles of calcium carbonate precipitate are evenly dispersed in the slurry along with the polyvinyl alcohol and sodium carboxymethyl cellulose, and the resulting slurry has good viscosity.

[0022] Preferably, the viscosity of the coating used in the coating layer is 800mPa*S to 1200mPa*S, and the solid content is 60% to 65%. In the present invention, the sodium chloride generated by the precipitation reaction effectively increases the viscosity of the obtained coating slurry.

[0023] Preferably, the drying process conditions in step S2 are as follows: drying at 90° C. to 120° C. for 20 to 30 seconds.

[0024] The preferred process parameters for calendering in step S3 are as follows:

[0025] The temperature is 100°C to 120°C, and the pressure is 20 kN / m to 40 kN / m.

[0026] Another object of the present invention is to provide a coated white board paper, wherein the whiteness, glossiness and ink absorption rate of the coated white board paper obtained by the present invention are significantly improved.

[0027] To solve this technical problem, the technical solution of the present invention is:

[0028] Provided is a coated white board paper prepared according to the preparation method provided by the present invention.

[0029] Preferably, it includes coated paper and a coating layer, wherein the coating layer is bonded to the coated paper, and the coating layer includes kaolin, calcium carbonate with a hollow spherical structure, polyvinyl alcohol as an adhesive, and sodium carboxymethyl cellulose as a dispersant along the thickness direction of the coating, wherein the calcium carbonate is distributed along the chain structure of the polyvinyl alcohol and the surface of the sodium carboxymethyl cellulose; the calcium carbonate distributed along the chain structure of the polyvinyl alcohol between the flaky kaolin and the spherical calcium carbonate distributed around the sodium carboxymethyl cellulose together form a connecting space between the ink absorption channels to form the ink absorption channels.

[0030] By adopting the above technical solution, the beneficial effects of the present invention are:

[0031] The invention discloses an efficient coating process for coating white board paper. The main inventive concept is to use kaolin and calcium carbonate as pigments in combination, and in the process of mixing, calcium carbonate particles are distributed around polyvinyl alcohol as a binder and sodium carboxymethyl cellulose as a dispersant, and calcium ions in calcium chloride used for generating calcium carbonate are chelated with polyvinyl alcohol and sodium carboxymethyl cellulose respectively, which reduces the concentration of calcium ions in the coating slurry and controls the dispersion of calcium carbonate in the slurry; when sodium carbonate solution is added, the calcium ion concentration in the solution is low, and the nanoparticles formed by precipitation reaction are Calcium carbonate is inhibited by concentration and is difficult to stack and grow further, thus ensuring that calcium carbonate is evenly dispersed in the slurry; accompanied by calendering, the flaky kaolin rolls and shifts relative to the calcium carbonate particles or hollow calcium carbonate balls under the action of pressure, thereby ensuring that the obtained coating is flat while still retaining the connecting channels for absorbing ink. Since small particles or calcium carbonate particles with a hollow structure are dispersed around the connecting channels, the small size effect and large specific surface area of ​​the calcium carbonate particles can provide better ink absorption performance and promote the absorption and distribution of ink;

[0032] The hollow spherical calcium carbonate particles in the slurry used in the present invention not only improve the water retention and ink absorption performance, but also are effectively controlled by the squeezing and guiding effects of coating and calendering on the coating during the coating process. The obtained coating of the coated whiteboard paper effectively maintains microporosity. While kaolin and calcium carbonate are stacked to form a tight coating structure, sufficient pores are retained, which is beneficial to the absorption of ink. In the present invention, calcium carbonate is formed by calcium ions chelated with polyvinyl alcohol and CMC respectively, which effectively avoids surface closure caused by the strong interaction between PVA and pigment ions in the paper and the small volume of the formed coating voids. At the same time, the flaky kaolin in the present invention, the calcium carbonate distributed along the polyvinyl alcohol and the hollow calcium carbonate balls formed by surrounding the CMC form a structural coating layer with connected pores. The pigment particles in the coating layer are regularly stacked. The obtained coating of the coated whiteboard paper has improved smoothness and uniformity, improved the uniform absorption of ink on the paper surface, and improved printing quality and image clarity. DETAILED DESCRIPTION

[0033] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0034] Example 1

[0035] This embodiment discloses an efficient coating process for coating white board paper, comprising the following steps:

[0036] S1. Apply the coating on the surface of the coated paper using a coating machine, and the coating amount of the coating layer is shown in Table 1;

[0037] The pigment in the coating includes kaolin and calcium carbonate, wherein the calcium carbonate is in-situ generated during the mixing process of the coating, and the calcium carbonate particles are generated along the polyvinyl alcohol chain structure and the hollow spherical structure calcium carbonate is generated around the sodium carboxymethyl cellulose, and the calcium carbonate is evenly dispersed between the kaolin particles; the gaps between the flaky kaolin and the calcium carbonate particles are connected with the hollow spherical structure of the calcium carbonate to form absorption channels for the ink;

[0038] S2, drying the coated paper coated with the coating layer; the drying process conditions of step S2 are shown in Table 1.

[0039] S3, calendering and finishing the dried coated white board paper, during the calendering process, kaolin is relatively displaced and slid above and below the calcium carbonate hollow spheres and / or calcium carbonate particles, to obtain the target coated white board paper.

[0040] The process parameters of calendering in step S3 are shown in Table 1.

[0041] The coating composition used for coating the white paper in this embodiment is shown in Table 2 according to the mass fraction.

[0042] In this embodiment, the cationic color fixing agent is poly(dimethylaminoethyl acrylate) quaternary ammonium chloride.

[0043] The pigment in the present invention comprises kaolin and calcium carbonate, wherein kaolin is the main component, and the calcium carbonate generated in situ in the coating slurry is uniformly generated through a precipitation reaction, and the sodium chloride generated at the same time acts as an inorganic thickener to improve the viscosity of the obtained slurry, while avoiding the aggregation of polyvinyl alcohol molecular chains caused by the salting-out effect due to the generation of sodium chloride, thereby affecting the rheological properties and construction properties of the coating.

[0044] The preparation method of the coating in this embodiment comprises the following steps:

[0045] S11, calcium chloride, polyvinyl alcohol, carboxymethyl cellulose, cationic color fixing agent and defoaming agent are mixed evenly according to the target mass fractions; the carboxyl group of sodium carboxymethyl cellulose and polyvinyl alcohol are mixed with Ca 2+ Chelation;

[0046] S12, adding kaolin according to the mass fraction into the slurry obtained in S11 and stirring evenly;

[0047] S13, add calcium chloride solution in an amount equal to that of sodium carbonate to the mixture in S12, stir at a constant speed, and CaCl 2 and Na 2 CO 3 Precipitation reactions occur around sodium carboxymethylcellulose and polyvinyl alcohol between kaolin particles;

[0048] The process conditions of constant stirring in S13 are shown in Table 2;

[0049] S14, adding deionized water to adjust the solid content of the obtained coating to obtain the target coating.

[0050] The viscosity of the coating used in the coating layer of this embodiment is 800mPa*S to 1200mPa*S, and the solid content is 60% to 65%, as shown in Table 2. The sodium chloride generated by the precipitation reaction in the present invention effectively increases the viscosity of the obtained coating slurry.

[0051] The coated white board paper prepared in this embodiment includes coated paper and a coating layer, wherein the coating layer is bonded to the coated paper, and the coating layer includes kaolin, calcium carbonate with a hollow spherical structure, polyvinyl alcohol as an adhesive, and sodium carboxymethyl cellulose as a dispersant along the thickness direction of the coating layer, wherein the calcium carbonate is distributed along the chain structure of the polyvinyl alcohol and the surface of the sodium carboxymethyl cellulose; the calcium carbonate distributed along the chain structure of the polyvinyl alcohol between the flaky kaolin and the spherical calcium carbonate distributed around the sodium carboxymethyl cellulose together form a connecting space between the ink absorption channels to form an ink absorption channel.

[0052] Example 2

[0053] The main differences between this embodiment and embodiment 1 are shown in Table 1 and Table 2.

[0054] Example 3

[0055] The main differences between this embodiment and embodiment 1 are shown in Table 1 and Table 2.

[0056] Example 4

[0057] The main differences between this embodiment and embodiment 1 are shown in Table 1 and Table 2.

[0058] Table 1 High efficiency coating process parameters in Examples 1 to 4

[0059]

[0060] Table 2 Composition (mass fraction) and preparation parameters of coatings in Examples 1 to 4 and Comparative Examples

[0061]

[0062]

[0063] Comparative Example

[0064] This comparative example discloses an efficient coating process for coating white board paper. The main difference between this comparative example and Example 3 is that the coating composition used in this comparative example includes the following substances in parts by mass:

[0065]

[0066] The calcium carbonate particles in this comparative example are commercially available calcium carbonate, and the specific parameters are D50≤12 μm and purity≥98%.

[0067] Add the above components according to their mass fractions into deionized water and stir to mix evenly, and add deionized water to adjust the viscosity to 1056mPa*s;

[0068] The coating process conditions of this comparative example are the same as those of Example 3, and coated white board paper is obtained.

[0069] The K&N ink absorption test, the roughness, smoothness and glossiness of the coating surface of the coated whiteboard paper obtained in Examples 1 to 4 and the comparative example were tested respectively, as shown in Table 3 for details.

[0070] Table 3 Properties of coated whiteboard paper obtained in Examples 1 to 4 and Comparative Examples

[0071]

[0072] As shown in Table 3, the K&N value of the coated white board paper obtained by the present invention is significantly improved, while maintaining good glossiness and low roughness.

[0073] The main inventive concept of the present invention is to use kaolin and calcium carbonate as a pigment in combination, and in the process of mixing, calcium carbonate particles are dispersed along the materials distributed around polyvinyl alcohol as a binder and sodium carboxymethyl cellulose as a dispersant, and calcium ions in calcium chloride used to generate calcium carbonate are chelated with polyvinyl alcohol and sodium carboxymethyl cellulose respectively, which reduces the concentration of calcium ions in the coating slurry and controls the dispersion of calcium carbonate in the slurry; when sodium carbonate solution is added, the calcium ion concentration in the solution is low, and the nanoparticles of calcium carbonate formed by the precipitation reaction are inhibited by the concentration and are difficult to stack and further grow, thereby ensuring the uniform dispersion of calcium carbonate in the slurry; and its accompanying With calendering, the flaky kaolin is subjected to pressure to roll and shift relative to the calcium carbonate particles or hollow calcium carbonate balls, so that the connected channels for absorbing ink are still retained under the premise of ensuring the flatness of the obtained coating. Since small particles or calcium carbonate particles with a hollow structure are dispersed around the connected channels, due to the small size effect and large specific surface area of ​​the calcium carbonate particles, better ink absorption performance can be provided, and the absorption and distribution of ink are promoted; the present invention utilizes the combination of calcium carbonate with suitable particle size generated in the process of mixing and flaky kaolin to improve the smoothness and uniformity of the coating, improve the uniform absorption of ink on the surface of paper, and improve the printing quality and image clarity. The mass fraction of the calcium carbonate precipitate generated in situ in Example 4 is greater than that of Examples 1, 2 and 3, and the excessive sodium chloride generated is not conducive to the gloss and roughness of the coating; the micron particles used in the comparative example have a small specific surface area and it is difficult to improve the ink absorption performance of the obtained coating layer, and the general nano calcium carbonate is difficult to disperse directly added to the mixture due to its own high surface energy, and the high specific surface area of ​​the nano material is difficult to apply.

Claims

1. An efficient coating process for coating white board paper, characterized in that: The following steps are involved: S1, applying the coating on the surface of the coated paper using a coating machine; The pigment in the coating includes kaolin and calcium carbonate, wherein the calcium carbonate is in-situ generated during the mixing process of the coating, and the calcium carbonate particles are generated along the polyvinyl alcohol chain structure and the hollow spherical structure calcium carbonate is generated around the sodium carboxymethyl cellulose, and the calcium carbonate is evenly dispersed between the kaolin particles; the gaps between the flaky kaolin and the calcium carbonate particles are connected with the hollow spherical structure of the calcium carbonate to form absorption channels for the ink; S2, drying the coated paper coated with the coating layer; S3, calendering and finishing the dried coated white board paper, during the calendering process, kaolin is relatively displaced and slid above and below the calcium carbonate hollow spheres and / or calcium carbonate particles, to obtain the target coated white board paper.

2. The efficient coating process for coated white board paper according to claim 1, characterized in that: The coating composition used in the coating layer of coated white paper includes the following substances in parts by mass:

3. The efficient coating process for coated white board paper according to claim 2, characterized in that: The preparation method of the coating comprises the following steps: S11, calcium chloride, polyvinyl alcohol, carboxymethyl cellulose, cationic color fixing agent and defoaming agent are mixed uniformly according to the target mass fractions; the carboxyl group of sodium carboxymethyl cellulose and polyvinyl alcohol are mixed with Ca 2+ Chelation; S12, adding kaolin according to the mass fraction into the slurry obtained in S11 and stirring evenly; S13, adding a calcium chloride solution in an equal molar amount to the sodium carbonate to the mixture of S12, stirring at a constant speed, and CaCl2 and Na2CO3 undergo precipitation reaction around the sodium carboxymethyl cellulose and polyvinyl alcohol between the kaolin particles; S14, adding deionized water to adjust the solid content of the obtained coating to obtain the target coating.

4. The efficient coating process for coated white board paper according to claim 3, characterized in that: The process conditions for constant stirring in S13 are 800r / min to 1000r / min, and the stirring time is 45min to 65min.

5. The efficient coating process for coated white board paper according to claim 1, characterized in that: The coating material used for the coating layer has a viscosity of 800mPa*S to 1200mPa*S and a solid content of 60% to 65%.

6. The efficient coating process for coated white board paper according to claim 1, characterized in that: The drying process conditions in step S2 are as follows: drying at 90°C to 120°C for 20S to 30S.

7. The efficient coating process for coated white board paper according to claim 1, characterized in that: The process parameters of calendering in step S3 are as follows: The temperature is 100°C to 120°C, and the pressure is 20 kN / m to 40 kN / m.

8. A coated white board paper prepared according to the preparation method according to any one of claims 1 to 7.

9. The coated white board paper according to claim 8, characterized in that: The invention comprises coated paper and a coating layer, wherein the coating layer is bonded to the coated paper, and the coating layer comprises kaolin, calcium carbonate with a hollow spherical structure, polyvinyl alcohol as an adhesive, and sodium carboxymethyl cellulose as a dispersant along the thickness direction of the coating layer, wherein the calcium carbonate is distributed along the chain structure of the polyvinyl alcohol and the surface of the sodium carboxymethyl cellulose; the calcium carbonate distributed along the chain structure of the polyvinyl alcohol between the flaky kaolin and the spherical calcium carbonate distributed around the sodium carboxymethyl cellulose together form a connecting space between the ink absorption channels to form the ink absorption channels.

Citation Information

Patent Citations

  • Crosslinked polyurea hollow microspheres and preparation method and application thereof

    CN105801898A

  • White board paper suitable for high-speed printing and preparation method of white board paper

    CN109972446A

  • Preparation process of coating layer of coated grey-bottom white board

    CN116892130A

  • Modified amorphous calcium carbonate, preparation method thereof and cellulose composite paper

    CN118005062A

  • Coated paper for inkjet printing

    JP2016049744A