Hydrogen sensor and preparation method thereof

By using the combined structure of SnO2 layer, palladium particle layer, polymer layer and gaschromic layer in the hydrogen sensor, the problem of insufficient selectivity and practicality of the existing hydrogen sensor is solved, and hydrogen detection with high selectivity and rapid response is achieved. .

CN118731007APending Publication Date: 2024-10-01ZHENGZHOU UNIVERSITY OF LIGHT INDUSTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310321980.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing hydrogen sensors have poor selectivity and low practicability, making it difficult to effectively detect hydrogen leaks and affecting the safety of hydrogen energy.

Method used

A hydrogen sensor structure including a substrate, a SnO2 layer, a palladium particle layer, a polymer layer and a gaschromic layer is adopted. The electrode layer is spaced between the palladium particle layer and the polymer layer or between the SnO2 layer and the polymer layer. The palladium particle layer is used and aerochromic layer to improve the selectivity and sensitivity of hydrogen detection.

Benefits of technology

It achieves high selectivity, sensitivity and fast response time, and improves the accuracy and stability of hydrogen leakage through dual signal detection of color changes and electrical signals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731007A_ABST
    Figure CN118731007A_ABST
Patent Text Reader

Abstract

The invention relates to a hydrogen sensor and a preparation method thereof, and belongs to the technical field of gas detection. The hydrogen sensor comprises the substrate, the SnO2 layer, the palladium particle layer, the polymer layer and the gasochromic layer which are sequentially arranged in an attached mode, and when the hydrogen sensor is used for detecting hydrogen, good selectivity, high sensitivity and short response time and recovery time are achieved. The gasochromic layer can generate color change when detecting hydrogen, and meanwhile, the hydrogen sensor can generate an electric signal, so that the hydrogen leakage detection speed and accuracy can be improved, and the hydrogen leakage detection stability is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydrogen sensor and a preparation method thereof, belonging to the technical field of gas detection. Background Art

[0002] Gas sensors are an important branch of chemical sensors. With the development of science and technology, the scale of industrial and agricultural production has gradually expanded, the types of products have continued to increase, and the role played by gas sensors in many aspects of production and life has become increasingly important. It has been widely used in many fields such as transportation, information technology, health care, industrial and agricultural production, environmental protection, aerospace, national defense and military, and even people's daily life.

[0003] The combustion product of hydrogen is water, which does not pollute the environment, is recyclable, and has high energy density. Therefore, it is called "the cleanest energy in the world" and is widely used in aerospace, electronic manufacturing, chemical production and other fields. However, hydrogen is extremely volatile and flammable (>4%), and it is colorless and odorless and difficult to be sensed by human senses. If it leaks, it will pose a huge threat to human safety. Therefore, it is very important to develop a new generation of room temperature hydrogen detectors with high selectivity, high sensitivity and fast response speed to ensure the safety of hydrogen energy. For example, Chinese patent document CN 115541661A discloses a hydrogen sensor based on ohmic contact at room temperature and a preparation method thereof, wherein the hydrogen sensor includes a substrate, a gate electrode, a gate insulating layer, a semiconductor layer, a source electrode and a drain electrode arranged in sequence from bottom to top, and a hydrogen sensitive array, a source electrode and a drain electrode are provided on the upper surface of the semiconductor layer, and the hydrogen sensitive array is located between the source electrode and the drain electrode, and the hydrogen sensitive array is doped with metal elements. However, the hydrogen sensor has poor selectivity for hydrogen, and needs to be judged by voltage changes during detection, which has poor practicality and low reliability. Summary of the invention

[0004] The purpose of the present invention is to provide a hydrogen sensor which can solve the problems of poor selectivity and poor practicality of current hydrogen sensors.

[0005] Another object of the present invention is to provide a method for preparing a hydrogen sensor, which can solve the problem that the hydrogen sensor prepared by the current method for preparing a hydrogen sensor has poor selectivity and poor practicality.

[0006] In order to achieve the above objectives, the technical solution adopted by the hydrogen sensor of the present invention is:

[0007] A hydrogen sensor, comprising a substrate, a SnO2 layer, a palladium particle layer, a polymer layer and a gas-induced color-changing layer which are sequentially laminated; the polymer layer is a polymethyl methacrylate layer;

[0008] The hydrogen sensor further includes an electrode layer; the electrode layer is spaced between the palladium particle layer and the polymer layer; or the electrode layer is spaced between the SnO2 layer and the polymer layer, and the palladium particle layer is located between the spaced electrode layers.

[0009] The hydrogen sensor of the present invention comprises a substrate, a SnO2 layer, a palladium particle layer, a polymer layer and a gas-induced color layer which are sequentially laminated and arranged, and has good selectivity, high sensitivity, short response time and recovery time when used to detect hydrogen. The gas-induced color layer will change when hydrogen is detected, and the hydrogen sensor will also generate an electrical signal, which can improve the speed and accuracy of hydrogen leak detection, thereby ensuring the stability of hydrogen leak detection.

[0010] Preferably, the thickness of the SnO2 layer is 3nm, and the thickness of the palladium particle layer is 4nm; or the thickness of the SnO2 layer is 5nm, and the thickness of the palladium particle layer is 2nm; or the thickness of the SnO2 layer is 8nm, and the thickness of the palladium particle layer is 2nm; or the thickness of the SnO2 layer is 11nm, and the thickness of the palladium particle layer is 3nm.

[0011] According to the applicant's extensive experimental research results, due to the small thickness of the palladium particle layer, the performance of the hydrogen sensor obtained when the electrode layer is spaced between the palladium particle layer and the polymer layer is close to that of the hydrogen sensor obtained when the electrode layer is spaced between the SnO2 layer and the polymer layer.

[0012] Preferably, the gasochromic layer is made of WO3-Pd-SiO2 sol. Preferably, the gasochromic layer is formed by coating the WO3-Pd-SiO2 sol and then drying it, and the coating is performed by spin coating, and the rotation speed of the spin coating is 300-600 rpm. For example, the rotation speed of the spin coating is 500 rpm. WO3 and Pd in ​​the gasochromic layer can react with hydrogen to improve the response strength of the hydrogen sensor.

[0013] Preferably, the WO3-Pd-SiO2 sol is prepared by a method comprising the following steps: adding PdCl2 to the WO3 sol, mixing until the PdCl2 is completely dissolved to obtain a WO3-Pd solution, and then adding silica sol to the WO3-Pd solution to obtain a WO3-Pd-SiO2 sol.

[0014] It is understood that the silica sol is a dispersion of nano-silicon dioxide in an organic solvent. Preferably, the organic solvent is propylene glycol methyl ether acetate. Preferably, the mass ratio of the silica sol to PdCl2 is (10-13):4. Preferably, the molar ratio of the Si element in the silica sol to the W element in the WO3 sol is (0.9-1):1. For example, the molar ratio of the Si element in the silica sol to the W element in the WO3 sol is 1:1.

[0015] Preferably, the WO3 sol is prepared by Kudo method. Preferably, the concentration of W element in the WO3 sol is 3-6 mol / L. For example, the concentration of W element in the WO3 sol is 5 mol / L.

[0016] Preferably, the WO3 sol is prepared by a method comprising the following steps: mixing tungsten powder and ethanol, then adding hydrogen peroxide, mixing for not less than 3 hours, separating the solid and liquid, and then mixing the liquid obtained by the solid-liquid separation at a temperature not lower than 80° C. to obtain the WO3 sol.

[0017] Preferably, the mass fraction of the hydrogen peroxide is 25-35%. For example, the mass fraction of the hydrogen peroxide is 30%.

[0018] Preferably, the volume of hydrogen peroxide corresponding to 5.4 g of tungsten powder is 20-40 mL. For example, the volume of hydrogen peroxide corresponding to 5.4 g of tungsten powder is 30 mL.

[0019] Preferably, the molar ratio of the Pd element in the PdCl2 to the W element in the WO3 sol is 1:(10-50). For example, the molar ratio of the Pd element in the PdCl2 to the W element in the WO3 sol is 1:50. Preferably, the mass ratio of the silica sol to PdCl2 is (10-13):4. For example, the mass ratio of the silica sol to PdCl2 is 10:4.

[0020] Preferably, the thickness of the gasochromic layer is 100-170 nm. If the thickness of the gasochromic layer is too small, the color change effect will be poor, and if the thickness is too large, the color change effect will be seriously delayed.

[0021] Preferably, the thickness of the polymer layer is 30-70 nm. If the thickness of the polymer layer is too small, the selectivity of the hydrogen sensor to detect hydrogen will be poor, and if the thickness is too large, the gas selectivity will be excessive, resulting in reaction hysteresis.

[0022] In order to improve the adhesion of the electrode layer on the palladium particle layer or the SnO2 layer, preferably, the electrode layer includes a transition layer and a conductive layer, the transition layer is a Ti layer or a Cr layer; the electrode layer is arranged between the palladium particle layer and the polymer layer, and the electrode layer is arranged on the palladium particle layer through the transition layer; or the electrode layer is arranged between the SnO2 layer and the polymer layer, and the electrode layer is arranged on the SnO2 layer through the transition layer.

[0023] Preferably, the thickness of the transition layer is 2-3 nm. If the thickness of the transition layer is too small, the effect of improving the adhesion of the electrode layer on the palladium particle layer or the SnO2 layer will fail.

[0024] Preferably, the thickness of the conductive layer is 5-10 nm. If the thickness of the conductive layer is too small, the conductivity will be poor, and if the thickness is too large, the polymer layer will not be able to effectively wrap the electrode layer, resulting in poor selectivity of the hydrogen sensor in detecting hydrogen.

[0025] It can be understood that the conductive layer is made of conductive metal, and preferably, the conductive layer is an Au layer.

[0026] In the present invention, when the electrode layer is arranged between the palladium particle layer and the polymer layer, the thickness of the polymer layer refers to the distance between one side of the polymer layer in contact with the gasochromic layer and the other side of the polymer layer (the side of the polymer layer in contact with the palladium particle layer); when the electrode layer is arranged between the SnO2 layer and the polymer layer, and the palladium particle layer is located between the electrode layers arranged at intervals, the thickness of the polymer layer refers to the distance between one side of the polymer layer in contact with the gasochromic layer and the other side of the polymer layer (the side of the polymer layer in contact with the palladium particle layer).

[0027] The technical solution adopted by the method for preparing the hydrogen sensor of the present invention is:

[0028] A method for preparing a hydrogen sensor as described above comprises the following steps: coating a SnO2 precursor solution on a substrate, forming a SnO2 layer after drying, then depositing a palladium particle layer on the SnO2 layer, then depositing an electrode layer on the palladium particle layer at intervals, then coating a polymer solution on the electrode layer and the palladium particle layer, forming a polymer layer after drying, and finally providing a gasochromic layer on the polymer layer;

[0029] Alternatively, a SnO2 precursor solution is coated on the substrate to form a SnO2 layer after drying, and then a palladium particle layer and an electrode layer are deposited on the SnO2 layer to form spaced electrode layers, with the palladium particle layer located between the spaced electrode layers, and then a polymer solution is coated on the palladium particle layer and the electrode layer to form a polymer layer after drying, and finally a gasochromic layer is arranged on the polymer layer.

[0030] The method for preparing the hydrogen sensor of the present invention is simple to operate and provides an effective way to develop a strong, flexible, transparent and durable hydrogen sensor.

[0031] Preferably, the SnO2 precursor solution is prepared by a method comprising the following steps: mixing 2-methoxyethanol and stannous chloride dihydrate until the stannous chloride dihydrate is completely dissolved, and separating the solid and the liquid to obtain a stannous chloride dihydrate solution, i.e., the SnO2 precursor solution. Preferably, the concentration of the stannous chloride dihydrate solution is 0.025 to 0.1 mol / L. Preferably, the coating of the SnO2 precursor solution is performed by spin coating, and the rotation speed of the spin coating is 1500 to 3000 rpm. For example, the coating of the SnO2 precursor solution is performed by spin coating, and the rotation speed of the spin coating is 3000 rpm.

[0032] Preferably, a palladium particle layer is deposited on the SnO2 layer by thermal evaporation deposition at a deposition rate of

[0033] Preferably, the polymethyl methacrylate solution is an anisole solution of polymethyl methacrylate. Preferably, the weight average molecular weight of the polymethyl methacrylate is 200000 to 350000. Preferably, the concentration of the polymethyl methacrylate solution is 35 to 45 mg / mL. For example, the concentration of the polymethyl methacrylate solution is 40 mg / mL.

[0034] Preferably, the coating of the polymer solution is performed by spin coating, and the rotation speed of the spin coating is 3000-4000 rpm. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the thickness test results of SnO2 thin films prepared from SnO2 precursor solutions with different concentrations by X-ray reflection in Experimental Example 1;

[0036] Figure 2 This is a schematic diagram of the results of characterizing the surface morphology of a SnO2 film with a thickness of 11 nm in Experimental Example 2; wherein, Figure 2 a is the SEM image, Figure 2 b is the AFM image, Figure 2 c is the analysis diagram of surface roughness;

[0037] Figure 3 A high-resolution transmission electron microscope (HR-TEM) cross-sectional image of the Pd nanoparticle layer in Experimental Example 2 and a schematic diagram of the elemental composition analysis results;

[0038] Figure 4 Schematic diagram of the X-ray photoelectron spectroscopy test results of the film before and after palladium deposition in Experimental Example 2; wherein, Figure 4a is the high-resolution Sn3d XPS spectrum of SnO2 thin film. Figure 4 b is the high-resolution O1s XPS spectrum of SnO2 thin film. Figure 4 c is the high-resolution O1s XPS spectrum of the SnO2 film after deposition of the Pd nanoparticle layer;

[0039] Figure 5 The schematic diagram is a dynamic response diagram of the sensor of SnO2 film with different thickness and palladium nanoparticle with different thickness in Experimental Example 3 at room temperature, 2% hydrogen content in the air and 0.1V bias voltage; wherein, Figure 5 a is a schematic diagram of the dynamic response of the sensor with a SnO2 film thickness of 3nm and palladium nanoparticles of different thicknesses. Figure 5 b is a schematic diagram of the dynamic response of the sensor with SnO2 film thickness of 8nm and palladium nanoparticles of different thicknesses. Figure 5 c is a schematic diagram of the dynamic response of the sensor with SnO2 film thickness of 11nm and palladium nanoparticles of different thicknesses. Figure 5 d is a schematic diagram of the dynamic response of the sensor with SnO2 film having a thickness of 5 nm and palladium nanoparticles of different thicknesses;

[0040] Figure 6 Schematic diagram of the initial resistance test results of the sensor with SnO2 films of different thicknesses and Pd particle layers of different thicknesses in Experimental Example 3; wherein, Figure 6 a is a schematic diagram of the initial resistance of the sensor with a SnO2 film thickness of 3 nm and palladium nanoparticles of different thicknesses. Figure 6 b is a schematic diagram of the initial resistance of the sensor with SnO2 film thickness of 5nm and palladium nanoparticles of different thicknesses. Figure 6 c is a schematic diagram of the initial resistance of the sensor with SnO2 film thickness of 8nm and palladium nanoparticles of different thicknesses. Figure 6 d is a schematic diagram of the initial resistance of the sensor with SnO2 film having a thickness of 11 nm and palladium nanoparticles of different thicknesses;

[0041] Figure 7 TEM images of palladium nanoparticles with thicknesses of 1 nm, 3 nm, 5 nm, and 10 nm in Experimental Example 3; wherein, Figure 7 a is the TEM image of the palladium nanoparticle layer with a thickness of 1 nm when the thickness of the SnO2 film is 3 nm. Figure 7 b is the TEM image of the palladium nanoparticle layer with a thickness of 3 nm when the thickness of the SnO2 film is 3 nm. Figure 7 c is the TEM image of the SnO2 film with a thickness of 3 nm and a palladium nanoparticle layer with a thickness of 5 nm. Figure 7d is the TEM image of the SnO2 film with a thickness of 3 nm and a palladium nanoparticle layer with a thickness of 10 nm. Figure 7 e is the HRTEM image of the palladium nanoparticle layer with a thickness of 3 nm when the thickness of the SnO2 film is 3 nm;

[0042] Figure 8 It is a schematic diagram of the detection result of the sensor with a SnO2 film thickness of 3nm and a palladium nanoparticle thickness of 4nm in Experimental Example 4 for hydrogen gas with a content of 20ppm to 2% in the air;

[0043] Fig. 9 It is a schematic diagram of the result of the sensor with a SnO2 film thickness of 8nm and a palladium nanoparticle thickness of 2nm detecting hydrogen gas with a content of 20ppm to 2% in the air in Experimental Example 4;

[0044] Fig.10 It is a schematic diagram of the detection result of the sensor with a SnO2 film thickness of 11nm and a palladium nanoparticle thickness of 3nm in Experimental Example 4 for hydrogen gas with a content of 20ppm to 2% in the air;

[0045] Fig.11 It is a schematic diagram of the result of the sensor with a SnO2 film thickness of 5nm and a palladium nanoparticle thickness of 2nm detecting hydrogen gas with a content of 20ppm to 2% in the air in Experimental Example 4;

[0046] Fig.12 This is a schematic diagram of the test results of the transmittance and resistance response of the hydrogen sensor of Example 6 in Experimental Example 5 in air with different hydrogen contents; wherein, Fig.12 a is a schematic diagram of the transmittance and resistance response test results of the hydrogen sensor of Example 6 in air with a hydrogen content of 0.5%, Fig.12 b is a schematic diagram of the transmittance and resistance response test results of the hydrogen sensor of Example 6 in air with a hydrogen content of 1%, Fig.12 c is a schematic diagram of the transmittance and resistance response test results of the hydrogen sensor of Example 6 in air with a hydrogen content of 4%. DETAILED DESCRIPTION

[0047] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0048] The raw materials used in Examples 9-16 of the present invention are as follows: tin (II) chloride dihydrate (>99.999%), tungsten powder, PdCl2, PMMA (average molar weight of 350,000), anisole purchased from Sigma Aldrich; 2-methoxyethanol (2ME) purchased from Samchun Chemical; transparent polyimide (PI) varnish purchased from Fafnie Korea; all chemicals were not further purified.

[0049] 1. The embodiments of the hydrogen sensor of the present invention are as follows:

[0050] Example 1

[0051] The hydrogen sensor of this embodiment includes a substrate, a SnO2 layer, a palladium particle layer, a polymer layer and a gas-induced chromic layer which are sequentially laminated; the polymer layer is a polymethyl methacrylate layer (PMMA layer), the hydrogen sensor also includes an electrode layer, the electrode layer is spaced between the palladium particle layer and the polymer layer, the electrode layer includes a transition layer and a conductive layer, the conductive layer is an Au layer, the transition layer is a Cr layer, and the electrode layer is arranged on the palladium particle layer through the transition layer;

[0052] In the hydrogen sensor of this embodiment, the substrate is a silicon wafer with a thermally grown SiO2 film on the surface, wherein the thickness of the silicon wafer is 1 mm, the thickness of the thermally grown SiO2 film is 300 nm, the SnO2 layer is disposed on the SiO2 film, the thickness of the SnO2 layer is 5 nm, the thickness of the palladium particle layer is 2 nm, the thickness of the transition layer is 2 nm, the thickness of the polymer layer is 30 nm, the thickness of the gasochromic layer is 100 nm, and the thickness of the conductive layer is 10 nm. In this embodiment, the thickness of the polymer layer refers to the distance between the side of the polymer layer that is attached to the palladium particle layer and the side of the polymer layer that is away from the palladium particle layer (the side of the polymer layer that is attached to the gasochromic layer).

[0053] Example 2

[0054] The hydrogen sensor of this embodiment is different from the hydrogen sensor of Embodiment 1 only in that, in the hydrogen sensor of this embodiment, the thickness of the SnO2 layer is 3 nm, the thickness of the palladium particle layer is 4 nm, the thickness of the polymer layer is 40 nm, and the thickness of the gas-chromic layer is 120 nm.

[0055] Example 3

[0056] The only difference between the hydrogen sensor of this embodiment and the hydrogen sensor of Embodiment 1 is that in the hydrogen sensor of this embodiment, the thickness of the SnO2 layer is 8 nm, the thickness of the palladium particle layer is 2 nm, the thickness of the polymer layer is 70 nm, and the thickness of the gas-chromic layer is 170 nm.

[0057] Example 4

[0058] The only difference between the hydrogen sensor of this embodiment and the hydrogen sensor of Example 1 is that in the hydrogen sensor of this embodiment, the thickness of the SnO2 layer is 11 nm, the thickness of the palladium particle layer is 3 nm, the thickness of the polymer layer is 60 nm, and the thickness of the gas-chromic layer is 150 nm.

[0059] Example 5

[0060] The hydrogen sensor of this embodiment is different from the hydrogen sensor of Embodiment 1 only in that, in the hydrogen sensor of this embodiment, the substrate is a polyimide film with a thickness of 800 nm.

[0061] Example 6

[0062] The only difference between the hydrogen sensor of this embodiment and the hydrogen sensor of Example 5 is that in the hydrogen sensor of this embodiment, the thickness of the SnO2 layer is 3 nm, the thickness of the palladium particle layer is 4 nm, the thickness of the polymer layer is 40 nm, and the thickness of the gas-chromic layer is 120 nm.

[0063] Example 7

[0064] The only difference between the hydrogen sensor of this embodiment and the hydrogen sensor of Embodiment 5 is that in the hydrogen sensor of this embodiment, the thickness of the SnO2 layer is 8 nm, the thickness of the palladium particle layer is 2 nm, the thickness of the polymer layer is 50 nm, and the thickness of the gas-chromic layer is 130 nm.

[0065] Example 8

[0066] The only difference between the hydrogen sensor of this embodiment and the hydrogen sensor of Example 5 is that in the hydrogen sensor of this embodiment, the thickness of the SnO2 layer is 11 nm, the thickness of the palladium particle layer is 3 nm, the thickness of the polymer layer is 60 nm, and the thickness of the gas-chromic layer is 170 nm.

[0067] 2. An embodiment of the method for preparing the hydrogen sensor of the present invention is as follows:

[0068] Example 9

[0069] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Embodiment 1, and specifically comprises the following steps:

[0070] (1) Preparation of SnO2 precursor solution: 2-methoxyethanol and stannous chloride dihydrate are mixed until the stannous chloride dihydrate is completely dissolved, and then filtered using a 0.2 μm polytetrafluoroethylene syringe filter to obtain a stannous chloride dihydrate solution with a concentration of 0.05 mol / L, which is the SnO2 precursor solution;

[0071] Preparation of WO3-Pd-SiO2 sol: WO3 sol was prepared by Kudo method. The specific method is as follows: 20 mL of ethanol was added to a beaker containing 5.4 g of tungsten powder under stirring, and then the beaker was placed in an ice bath. Then 30 mL of 30% hydrogen peroxide was added dropwise to the beaker. After the addition was completed, it was stirred for 3 h to obtain a transparent yellow mixture, and then centrifuged for 1 h. The supernatant obtained by centrifugation was stirred at 80 ° C until the solution turned into a transparent orange color. Then, the transparent orange solution was diluted with ethanol to obtain WO3 sol. The concentration of W element in WO3 sol 5 mol / L, then adding PdCl2 (the molar ratio of the Pd element in PdCl2 to the W element in WO3 sol is 1:50) as a catalyst to the WO3 sol, stirring until the PdCl2 is completely dissolved to obtain a WO3-Pd solution, and then adding silica sol to the WO3-Pd solution (the mass ratio of the silica sol to PdCl2 is 10:4, the molar ratio of the Si element in the added silica sol to the W element in the WO3 sol is 1:1, and the silica sol is a dispersion of nano-silicon dioxide in propylene glycol methyl ether acetate) to obtain a WO3-Pd-SiO2 sol;

[0072] Preparation of PMMA solution: PMMA with a weight average molecular weight of 350,000 was added to anisole and stirred at 60°C for 6 h to obtain a 40 mg / mL PMMA solution;

[0073] (2) Preparation of hydrogen sensor: A substrate (a silicon wafer with a thermally grown SiO2 film on the surface, wherein the thickness of the silicon wafer is 1 mm and the thickness of the thermally grown SiO2 film is 300 nm) is cleaned with deionized water, acetone and isopropanol, respectively, and then cleaned with UV / ozone; a SnO2 precursor solution is spin-coated on the SiO2 film of the cleaned substrate at a speed of 3000 rpm for 60 seconds, and then the substrate coated with the SnO2 precursor solution is pre-baked at 100°C for 5 minutes, and then directly placed on a hot plate and heated in air at 400°C for 1 hour to form a SnO2 film on the SiO2 film of the substrate; then a thermal evaporation method is used on the SnO2 film to A palladium particle catalyst is deposited at a rate of, and then an electrode layer is deposited on the palladium catalyst layer by a thermal evaporation method. The electrode layer is arranged at intervals on the palladium catalyst layer. The electrode layer includes a Cr layer with a thickness of 2 nm and an Au layer with a thickness of 10 nm. The Cr layer serves as a transition layer to improve the adhesion of the Au layer on the palladium particle catalyst layer. The Au layer is a conductive layer, serving as a source and a drain. Finally, a PMMA solution is spin-coated on the electrode layer and the palladium particle catalyst layer (the portion not covering the electrode layer) at a rotation speed of 4000 rpm for 30 seconds, and then baked at 175°C for 10 minutes to form a PMMA layer, and then WO3-Pd-SiO2 sol is spin-coated on the PMMA layer at a rotation speed of 500 rpm for 60 seconds, and then dried at 60°C for 2 hours to form a gas-induced chromic layer on the PMMA layer.

[0074] Example 10

[0075] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Example 2. The difference between the preparation method of the hydrogen sensor of this embodiment and the preparation method of the hydrogen sensor of Example 9 is that the SnO2 precursor solution used in the preparation method of the hydrogen sensor of this embodiment is a stannous chloride dihydrate solution with a concentration of 0.025 mol / L.

[0076] Embodiment 11

[0077] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Example 3. The difference between the preparation method of the hydrogen sensor of this embodiment and the preparation method of the hydrogen sensor of Example 9 is that the SnO2 precursor solution used in the preparation method of the hydrogen sensor of this embodiment is a stannous chloride dihydrate solution with a concentration of 0.075 mol / L.

[0078] Example 12

[0079] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Example 4. The difference between the preparation method of the hydrogen sensor of this embodiment and the preparation method of the hydrogen sensor of Example 9 is that the SnO2 precursor solution used in the preparation method of the hydrogen sensor of this embodiment is a stannous chloride dihydrate solution with a concentration of 0.1 mol / L.

[0080] Embodiment 13

[0081] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Embodiment 5, and specifically comprises the following steps:

[0082] (1) This step is the same as step (1) of the method for preparing the hydrogen sensor of Example 9;

[0083] (2) A substrate (a silicon wafer with a thermally grown SiO2 film on the surface, wherein the thickness of the silicon wafer is 1 mm and the thickness of the thermally grown SiO2 film is 300 nm) is cleaned with deionized water, acetone, and isopropanol, respectively, and then cleaned with UV / ozone; a transparent polyimide (PI) varnish is then spin-coated onto the SiO2 film of the cleaned substrate at a speed of 1000 rpm for 30 seconds, and then the substrate coated with the transparent polyimide (PI) varnish is heated to a certain temperature at a heating rate of 2°C / min for annealing to form a PI layer on the SiO2 film. In order to avoid The PI film was wrinkled, and a staged annealing treatment was adopted. The substrate coated with transparent polyimide (PI) varnish was first heated to 60°C, kept warm for 30 minutes, then heated to 80°C, kept warm for 30 minutes, then heated to 150°C, kept warm for 30 minutes, then heated to 230°C, kept warm for 60 minutes, and finally heated to 300°C and cooled to room temperature; then the SnO2 precursor solution was spin-coated on the PI layer at a speed of 3000 rpm, the spin-coating time was 60 seconds, and then heated at 280°C for 4 hours to form a SnO2 film on the PI layer, and then the SnO2 film was thermally evaporated by a method to form a SnO2 film on the SnO2 film. A palladium particle catalyst is deposited at a rate of , and then an electrode layer is deposited on the palladium catalyst layer by a thermal evaporation method. The electrode layer is arranged at intervals on the palladium catalyst layer. The electrode layer includes a Cr layer with a thickness of 2 nm and an Au layer with a thickness of 10 nm. The Cr layer serves as a transition layer to improve the adhesion of the Au layer on the palladium particle catalyst layer. The Au layer is a conductive layer, serving as a source and a drain. Then, a PMMA solution is spin-coated on the electrode layer and the palladium catalyst layer (the portion not covering the electrode layer) at a rotation speed of 4000 rpm for 30 seconds, and then baked at 175°C for 10 minutes to form a PMMA layer on the electrode layer and the palladium catalyst layer. Finally, a WO3-Pd-SiO2 sol is spin-coated on the PMMA layer at a rotation speed of 500 rpm for 60 seconds, and then dried at 60°C for 2 hours to form a gas-induced chromic layer on the PMMA layer. Then, the PI layer is separated from the substrate to obtain a transparent flexible hydrogen sensor.

[0084] Embodiment 14

[0085] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Example 6. The difference between the preparation method of the hydrogen sensor of this embodiment and the preparation method of the hydrogen sensor of Example 13 is that the SnO2 precursor solution used in the preparation method of the hydrogen sensor of this embodiment is a stannous chloride dihydrate solution with a concentration of 0.025 mol / L.

[0086] Embodiment 15

[0087] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Example 7. The difference between the preparation method of the hydrogen sensor of this embodiment and the preparation method of the hydrogen sensor of Example 13 is that the SnO2 precursor solution used in the preparation method of the hydrogen sensor of this embodiment is a stannous chloride dihydrate solution with a concentration of 0.075 mol / L.

[0088] Example 16

[0089] The preparation method of the hydrogen sensor of this embodiment is the preparation method of the hydrogen sensor of Example 8. The difference between the preparation method of the hydrogen sensor of this embodiment and the preparation method of the hydrogen sensor of Example 13 is that the SnO2 precursor solution used in the preparation method of the hydrogen sensor of this embodiment is a stannous chloride dihydrate solution with a concentration of 0.1 mol / L.

[0090] Comparative Example 1

[0091] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that in the preparation method of the hydrogen sensor of this comparative example, when preparing the WO3-Pd-SiO2 sol, the concentration of the W element in the WO3 sol is 2 mol / L, and the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0092] Comparative Example 2

[0093] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that in the preparation method of the hydrogen sensor of this comparative example, when preparing the WO3-Pd-SiO2 sol, the concentration of the W element in the WO3 sol is 7 mol / L, and the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0094] Comparative Example 3

[0095] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that, in the preparation method of the hydrogen sensor of this comparative example, when preparing the WO3-Pd-SiO2 sol, the amount of silica sol (concentration remains unchanged) is adjusted so that the mass ratio of silica sol and PdCl2 is 9:4, and the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0096] Comparative Example 4

[0097] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that, in the preparation method of the hydrogen sensor of this comparative example, when preparing the WO3-Pd-SiO2 sol, the amount of silica sol (concentration remains unchanged) is adjusted so that the mass ratio of silica sol and PdCl2 is 14:4, and the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the gas-chromic layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0098] Comparative Example 5

[0099] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that in the preparation method of the hydrogen sensor of this comparative example, the molecular weight of PMMA used in preparing the PMMA solution is 100,000, and the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0100] Comparative Example 6

[0101] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that, in the preparation method of the hydrogen sensor of this comparative example, the molecular weight of PMMA used in preparing the PMMA solution is 400,000, and the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0102] Comparative Example 7

[0103] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that in the preparation method of the hydrogen sensor of this comparative example, the concentration of the PMMA solution is 30 mg / mL, and the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0104] Comparative Example 8

[0105] The only difference between the preparation method of the hydrogen sensor of this comparative example and the preparation method of the hydrogen sensor of Example 13 is that in the preparation method of the hydrogen sensor of this comparative example, the concentration of the PMMA solution is 50 mg / mL, and the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of this comparative example is the same as the thickness of the PMMA layer in the hydrogen sensor prepared by the preparation method of the hydrogen sensor of Example 13.

[0106] The instruments and methods used in the following experimental examples for testing the sensing performance of the hydrogen sensor are as follows: Agilent B15000A semiconductor parameter analyzer and MSTECH detection station with ELFLOW high-performance MFC were used to measure the current-voltage characteristics and gas sensing response. The sensor was placed in the gas test chamber below the gas pipe outlet and directly exposed to air containing a certain concentration of hydrogen. The sensor response is defined as I g / I a , where I g and I a The measured change current (i.e., the change in current after exposure to air containing a certain concentration of hydrogen) and the initial current are shown in Table 1. For all measurements, the applied voltage and temperature were 100 mV and 20°C, respectively.

[0107] Experimental Example 1

[0108] The performance and operating temperature of SMO-based sensors are strongly dependent on the thickness and morphology of the film, especially when the thickness of the film is at the nanometer level. In order to optimize the thickness of the SnO2 film, SnO2 films with a thickness of 3 to 11 nm were prepared by changing the concentration of the SnO2 precursor solution. The thickness of the SnO2 film prepared by SnO2 precursor solutions of different concentrations was studied by X-ray reflection. The results are shown in Figure 2. Figure 1 As shown in the figure, the root mean square roughness of SnO2 films with a thickness of 3 to 11 nm was analyzed by AFM and X-ray reflection method. Finally, the thickness and roughness of SnO2 films prepared from SnO2 precursor solutions with different concentrations were summarized and listed in Table 1.

[0109] Table 1 Thickness and RMS roughness of SnO2 films prepared from SnO2 precursor solutions with different concentrations

[0110] <![CDATA[Concentration of SnO2 precursor solution]]> <![CDATA[Thickness of SnO2 thin film]]> <![CDATA[Root mean square roughness of SnO2 thin film]]> 0.025mol / L 3nm 0.657nm 0.05mol / L 5nm 0.560nm 0.075mol / L 8nm 0.718nm 0.1mol / L 11nm 0.885nm

[0111] As shown in Table 1, the thickness of the SnO2 film increases proportionally with the concentration of the SnO2 precursor solution. The thickness of the prepared SnO2 film covers the Debye length of SnO2 (at 250°C, the Debye length of SnO2 is 3nm) to obtain a complete film that is completely electron depleted and extremely sensitive to environmental changes. When the thickness of the SnO2 film increases from 3nm to 11nm, the root mean square roughness of the SnO2 film increases from 0.657nm to 0.885nm.

[0112] Experimental Example 2

[0113] The surface morphology of SnO2 thin film with a thickness of 11nm was studied using high-resolution scanning electron microscopy (SEM) and atomic force microscopy (AFM). Figure 2 As shown, Figure 2 a is the SEM image, Figure 2 b is the AFM image, Figure 2 c is an analysis diagram of the surface roughness (i.e., a schematic diagram of the surface roughness tested under AFM).

[0114] from Figure 2 It can be seen that the grain size and distribution of SnO2 thin films are uniform, and the grains are well connected. The high quality of the film is mainly due to the use of suitable solvents to prepare the precursor, the use of optimized preparation process and relatively low heating film forming temperature.

[0115] At the same time, the 3nm thick palladium nanoparticle layer on the SnO2 film was characterized by high-resolution transmission electron microscopy (HR-TEM). The cross-sectional image of the palladium nanoparticle layer is shown in Figure 2. Figure 3 As shown in Figures 3a and 3b, the crystal planes with lattice spacing values ​​of 0.26nm and 0.33nm correspond to the (101) and (110) crystal planes of SnO2, respectively, and the crystal plane with a lattice spacing of 0.22nm corresponds to the Pd (111) crystal plane.

[0116] Finally, the elemental composition of the cross-section of the film after the deposition of the palladium nanoparticle layer was analyzed using energy dispersive X-ray spectroscopy. Figure 3 As shown in c, the results prove the existence and uniform distribution of Sn, O, and Pd in ​​the film.

[0117] X-ray photoelectron spectroscopy (XPS) was used to further investigate the chemical state and composition of the films before and after palladium deposition. Figure 4 a is the high-resolution Sn3d XPS spectrum of SnO2 film. Figure 4 It can be seen in a that the peaks at binding energies of 495.58 eV and 487.28 eV are attributed to Sn 3d3 / 2 and Sn 3d5 / 2 in SnO2, respectively; Figure 4 b is the high-resolution O1sXPS spectrum of SnO2 thin film. Figure 4 c is the high-resolution O1s XPS spectrum of the SnO2 film after the deposition of the Pd nanoparticle layer. Figure 4 b and Figure 4 c shows that the oxidation of the SnO2 thin film layer is fully within the normal range; from the Pd3d XPS spectrum of the Pd nanoparticle layer, it can be seen that the two deconvolution peaks at binding energies of 341.1eV and 335.81eV belong to Pd 33d / 2 and Pd 3d5 / 2 of metal Pd, respectively.

[0118] Experimental Example 3

[0119] In terms of metal catalyst decoration on SMO, most researchers focus on optimizing the catalyst dosage by fixing the thickness of SMO, but the actual situation is that the thickness and morphology of the SMO film need to be combined to optimize the catalyst dosage to improve the sensing performance.

[0120] In this experimental example, the preparation method of Example 9 is used to prepare a hydrogen sensor, except that WO3-Pd-SiO2 sol is not spin-coated on the PMMA layer, the thickness of the palladium particle layer in the prepared hydrogen sensor is 1-10nm, and the thickness of the SnO2 layer (SnO2 film) is 3nm, 5nm, 8nm and 11nm, respectively. The hydrogen sensor is then exposed to room temperature air (the hydrogen content in the air is 2%) to study the effects of the palladium particle layer thickness and the SnO2 layer thickness on the performance of the hydrogen sensor.

[0121] When the thickness of the SnO2 film in the sensor is 3nm, and the thickness of the palladium nanoparticles is 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10nm, respectively, the dynamic response of the sensor at room temperature, a hydrogen content (mass fraction) of 2% in the air, and a bias voltage of 0.1V is as follows: Figure 5 As shown in a.

[0122] When the thickness of the SnO2 film in the sensor is 8nm, and the thickness of the palladium nanoparticles is 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10nm, respectively, the dynamic response of the sensor at room temperature, a hydrogen content (mass fraction) of 2% in the air, and a bias voltage of 0.1V is as follows: Figure 5 As shown in b.

[0123] When the thickness of the SnO2 film in the sensor is 11nm, and the thickness of the palladium nanoparticles is 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10nm, respectively, the dynamic response of the sensor at room temperature, a hydrogen content (mass fraction) of 2% in the air, and a bias voltage of 0.1V is as follows: Figure 5 As shown in c.

[0124] When the thickness of the SnO2 film in the sensor is 5nm, and the thickness of the palladium nanoparticles is 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10nm, respectively, the dynamic response of the sensor at room temperature, a hydrogen content (mass fraction) of 2% in the air, and a bias voltage of 0.1V is as follows: Figure 5 As shown in d.

[0125] From the above test results, it can be seen that no matter how thick the SnO2 film is, after hydrogen exposure, the sensor response value will change significantly with the increase of the palladium nanoparticle thickness. And when the thickness of the SnO2 film in the sensor is 5nm and the deposition thickness of Pd is 2nm, the sensor response value is the largest. When the thickness of the SnO2 film in the sensor is constant, the corresponding Pd nanoparticle thickness has an optimal value. When the thickness of the SnO2 film in the sensor is 3nm, the optimal palladium nanoparticle thickness is 4nm; when the thickness of the SnO2 film in the sensor is 5nm, the optimal palladium nanoparticle thickness is 2nm; when the thickness of the SnO2 film in the sensor is 8nm, the optimal palladium nanoparticle thickness is 2nm; when the thickness of the SnO2 film in the sensor is 11nm, the optimal palladium nanoparticle thickness is 3nm. When the thickness of the Pd nanoparticle exceeds the optimal value, the sensor response decreases. The reason why SnO2 films of different thicknesses have different optimal Pd nanoparticle thicknesses is mainly due to the different surface roughness of SnO2 films of different thicknesses. The effective surface area of ​​palladium nanoparticles increases with the increase of SnO2 film surface roughness during deposition. The effective surface area of ​​palladium nanoparticles increases with the increase of SnO2 film surface roughness during deposition. When the surface roughness of SnO2 is high, the content of Pd nanoparticles deposited on the surface of SnO2 is large, and 3nm SnO2 is the optimal thickness to ensure the stability of current. Combined with the surface roughness, a 4nm Pd particle layer is selected as the optimal condition.

[0126] In order to further study the effect of the thickness of SnO2 film and Pd particle layer on the performance of the sensor (without gas-induced color layer), the initial resistance of the sensor with different thickness of SnO2 film and different thickness of Pd particle layer was tested. Figure 6 As shown, when the thickness of the SnO2 film in the sensor is 3nm, and the thickness of the palladium nanoparticles is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10nm, the initial resistance of the sensor is as follows: Figure 6 As shown in a, when the thickness of the SnO2 film in the sensor is 5 nm, and the thickness of the palladium nanoparticles is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is Figure 6As shown in (b), when the thickness of the SnO2 film in the sensor is 8 nm, and the thickness of the palladium nanoparticles is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is Figure 6 As shown in Figure c, when the thickness of the SnO2 film in the sensor is 11 nm, and the thickness of the palladium nanoparticles is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is Figure 6 As shown in d.

[0127] From the above test results, it can be seen that during thermal evaporation, Pd first forms scattered points and then gradually grows with the scattered points. When the evaporation thickness is low, the Pd scattered points are far apart, and only a few Pd grains are connected to form an electronic conduction path, resulting in a high resistance value. In addition, as the Pd thickness changes, the electrical conduction path of the sensor changes. When the Pd thickness is greater than the optimal value, the response values ​​of all sensors decrease.

[0128] At the same time, TEM was used to characterize the Pd-SnO2 films with different Pd nanoparticle thicknesses. When the thickness of the SnO2 film was 3nm, the TEM images of the palladium nanoparticle layer with thicknesses of 1nm, 3nm, 5nm, and 10nm were as follows: Figure 7 As shown, from Figure 7 It can be seen that the Pd nanoparticles are distributed on the surface of the SnO2 film. Before the optimal Pd thickness is reached, the Pd nanoparticles can only be transported through the SnO2 conduction pathway ( Figure 7 a. Figure 7 b and Figure 7 e); When the Pd thickness exceeds the optimum thickness, particle connection and agglomeration occur. This creates additional electron paths through the Pd layer, thus reducing the sensor response due to the effect on the sensor carrier modulation ( Figure 7 c and Figure 7 d).

[0129] Experimental Example 4

[0130] After obtaining the optimal SnO2 film thickness and Pd particle layer thickness, sensors with different SnO2 film thicknesses and corresponding optimal Pd particle layer thicknesses (without a gas-induced chromic layer, and the substrate is a silicon wafer with a surface thermally grown SiO2 film) were used to detect hydrogen in the air with a content (mass fraction) of 20ppm to 2%. The sensor was first exposed to room temperature air containing 0.002% hydrogen by mass, and the resistance response (I g / I a ), after the test results are stable, the hydrogen sensor is placed in room temperature air without hydrogen, and the resistance response (I g / I a), after the test results stabilized, the sensor was exposed to the next room temperature air containing a higher concentration of hydrogen and the test was repeated. The concentrations (mass fraction) of hydrogen were 0.002%, 0.005%, 0.01%, 0.025%, 0.05%, 0.08%, 0.1%, 0.5%, 0.8%, 1%, 1.5%, and 2%. When the thickness of the SnO2 film in the sensor was 3nm and the thickness of the palladium nanoparticles was 4nm, the test results were as follows: Figure 8 As shown in the figure, when the thickness of the SnO2 film in the sensor is 8nm and the thickness of the palladium nanoparticles is 2nm, the detection results are as follows Fig. 9 As shown in the figure, when the thickness of the SnO2 film in the sensor is 11nm and the thickness of the palladium nanoparticles is 3nm, the detection results are as follows Fig.10 As shown in Figure 2, when the thickness of the SnO2 film in the sensor is 5nm and the thickness of the palladium nanoparticles is 2nm, the detection results are as follows: Fig.11 As shown in the above test results, when the thickness of the SnO2 film in the sensor is 5nm and the thickness of the palladium nanoparticles is 2nm, the sensor has the highest response value of 16623 when detecting 2% hydrogen in the air (mass fraction). This response value is higher than the response value of the hydrogen sensor disclosed in the prior art when detecting hydrogen at room temperature.

[0131] From the above test results, it can be seen that when the thickness of the SnO2 film in the sensor is 5nm and the thickness of the Pd nanoparticles is 2nm, the response value of the sensor when detecting hydrogen is the highest.

[0132] Experimental Example 5

[0133] Resistive or colorimetric hydrogen sensors are the most common types of hydrogen sensors and have been extensively studied. In this experimental example, as a proof of concept, a multi-structure dual-signal hydrogen sensor was fabricated for the first time by combining a resistive sensor and a colorimetric sensor into one device. This type of geometry enables the sensor to be installed near a pipe where hydrogen flows or at a point where hydrogen is prone to leak, and solves the problem of measurement differences due to the rapid diffusion of hydrogen.

[0134] In order to test the detection performance of the hydrogen sensor of the present invention, the hydrogen sensor of Example 6 (the thickness of the SnO2 layer is 5nm, the thickness of the palladium particle layer is 2nm) and the hydrogen sensors prepared by the preparation methods of the hydrogen sensors of Comparative Examples 1-8 were exposed to room temperature air containing hydrogen, and the hydrogen content (mass fraction) in the air was 0.5%, 1%, and 4%, and then the transmittance (color) and resistance response (I g / I a), after the test results are stable, the hydrogen sensor is placed in room temperature air without hydrogen, and the transmittance (color) and resistance response (I g / I a ), the test was repeated 5 times, and the test results of the hydrogen sensor of Example 6 are as follows Fig.12 As shown. Fig.12 It can be seen that the base transmittance of the gas-chromic layer in the hydrogen sensor of Example 6 in air is 59%. When the content (mass fraction) of hydrogen in the air is 0.5%, 1% and 4%, the transmittance (test transmittance) is 9.6%, 5.8% and 3.7% respectively. When the content (mass fraction) of hydrogen is 1%, the response value (I g / I a ) is 5320. Therefore, the hydrogen sensor of Example 6 can provide qualitative (color) and quantitative (resistance) responses for early leakage detection, thereby improving the safety and reliability of using hydrogen. When the hydrogen sensor of Example 6 without the gas-induced color layer is tested according to the above method, the response value (I g / I a ) is 1317. Therefore, since the gas chromic layer contains Pd and WO3 can also react to hydrogen, the response value of the hydrogen sensor of Example 6 when detecting hydrogen with a content (mass fraction) of 1% is larger.

[0135] Meanwhile, the test results of the hydrogen sensors of Example 6 and the hydrogen sensors prepared by the preparation methods of the hydrogen sensors of Comparative Examples 1-8 are summarized in Table 2.

[0136] Table 2 Detection performance of the hydrogen sensor of Example 6 and the hydrogen sensors prepared in Comparative Examples 1-8

[0137]

[0138] In addition, when hydrogen peroxide with a mass fraction of 20% and 35%, the volume of hydrogen peroxide corresponding to each 5.4g of tungsten powder is 20mL and 40mL, the molar ratio of Pd element in PdCl2 to W element in WO3 sol is 1:10 and 1:30, the mass ratio of silica sol and PdCl2 is 13:4, and the molar ratio of Si element in silica sol to W element in WO3 sol is 0.9:1 to prepare WO3-Pd-SiO2 sol, and the prepared WO3-Pd-SiO2 sol is used to prepare a hydrogen sensor, or when a PMMA solution with a concentration of 35 and 45 mg / mL is used to prepare a hydrogen sensor, when hydrogen in the air is detected according to the above method, the detection performance of the hydrogen sensor for hydrogen is similar to the detection performance of the hydrogen sensor for hydrogen in Example 6.

[0139] When the hydrogen sensors of Example 5 and Examples 7-8 are used to detect hydrogen in the air according to the above method, the detection performance of the hydrogen sensors for hydrogen is similar to the detection performance of the hydrogen sensor of Example 6 for hydrogen.

Claims

1. A hydrogen sensor, characterized in that: It comprises a substrate, a SnO2 layer, a palladium particle layer, a polymer layer and a gas-induced color-changing layer which are sequentially laminated; the polymer layer is a polymethyl methacrylate layer; The hydrogen sensor further includes an electrode layer; the electrode layer is spaced between the palladium particle layer and the polymer layer; or the electrode layer is spaced between the SnO2 layer and the polymer layer, and the palladium particle layer is located between the spaced electrode layers.

2. The hydrogen sensor according to claim 1, characterized in that: The gaseous chromic layer is made of WO3-Pd-SiO2 sol.

3. The hydrogen sensor according to claim 2, characterized in that: The WO3-Pd-SiO2 sol is prepared by a method comprising the following steps: adding PdCl2 to the WO3 sol, mixing until the PdCl2 is completely dissolved to obtain a WO3-Pd solution, and then adding silica sol to the WO3-Pd solution to obtain a WO3-Pd-SiO2 sol; the concentration of the W element in the WO3 sol is 3 to 6 mol / L; the mass ratio of the silica sol to PdCl2 is (10 to 13):4; the molar ratio of the Si element in the silica sol to the W element in the WO3 sol is (0.9 to 1):

1.

4. The hydrogen sensor according to claim 1, characterized in that: The thickness of the gasochromic layer is 100-170 nm.

5. The hydrogen sensor according to claim 1, characterized in that: The thickness of the polymer layer is 30-70 nm.

6. The hydrogen sensor according to claim 1, characterized in that: The weight average molecular weight of the polymethyl methacrylate in the polymethyl methacrylate layer is 200,000 to 350,000.

7. The hydrogen sensor according to claim 1, characterized in that: The thickness of the SnO2 layer is 3nm, and the thickness of the palladium particle layer is 4nm; or the thickness of the SnO2 layer is 5nm, and the thickness of the palladium particle layer is 2nm; or the thickness of the SnO2 layer is 8nm, and the thickness of the palladium particle layer is 2nm; or the thickness of the SnO2 layer is 11nm, and the thickness of the palladium particle layer is 3nm.

8. The hydrogen sensor according to any one of claims 1 to 7, characterized in that: The electrode layer includes a transition layer and a conductive layer, the transition layer is a Ti layer or a Cr layer; the electrode layer is arranged between the palladium particle layer and the polymer layer, and the electrode layer is arranged on the palladium particle layer through the transition layer; or the electrode layer is arranged between the SnO2 layer and the polymer layer, and the electrode layer is arranged on the SnO2 layer through the transition layer.

9. The hydrogen sensor according to claim 8, characterized in that: The thickness of the transition layer is 2-3 nm; the thickness of the conductive layer is 5-10 nm.

10. A method for preparing a hydrogen sensor according to any one of claims 1 to 9, characterized in that: The following steps are involved: A SnO2 precursor solution is coated on a substrate to form a SnO2 layer after drying, a palladium particle layer is deposited on the SnO2 layer, an electrode layer is deposited on the palladium particle layer at intervals, a polymer solution is coated on the electrode layer and the palladium particle layer to form a polymer layer after drying, and finally a gas-induced chromic layer is disposed on the polymer layer; Alternatively, a SnO2 precursor solution is coated on the substrate to form a SnO2 layer after drying, and then a palladium particle layer and an electrode layer are deposited on the SnO2 layer to form spaced electrode layers, with the palladium particle layer located between the spaced electrode layers, and then a polymer solution is coated on the palladium particle layer and the electrode layer to form a polymer layer after drying, and finally a gasochromic layer is arranged on the polymer layer.