Pipeline weak magnetic stress internal detection signal quantification research method under demagnetization effect
By establishing a mathematical model for pipeline weak magnetic stress detection under demagnetization effect, the problem of signal interference caused by demagnetization effect in weak magnetic stress detection is solved, the detection accuracy and efficiency are improved, and accurate analysis of weak magnetic signals and interference elimination are achieved.
Patent Information
- Application Number
- CN202310296187.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-01
AI Technical Summary
In long-distance oil and gas pipelines, weak magnetic stress detection technology is interfered by the demagnetization effect, which makes signal intensity changes and features difficult to collect and identify, affecting detection efficiency.
A mathematical model for the detection of weak magnetic stress in pipelines under the demagnetization effect was established. By introducing the demagnetization field as a secondary field source, combined with magnetic calculations and Maxwell's equations, the spatial distribution relationship between the weak magnetic signal and the demagnetization field was analyzed, and a finite element simulation model was used. Verify signal characteristics and eliminate demagnetization interference.
It improves the accuracy and detection efficiency of weak magnetic stress detection, clarifies the demagnetization interference characteristics, enhances signal analysis capabilities, and improves detection accuracy.
Smart Images

Figure FDA0004143251960000011 
Figure FDA0004143251960000012 
Figure FDA0004143251960000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of long-distance oil and gas pipeline internal detection, and relates to a quantitative research method for pipeline weak magnetic stress internal detection signals under demagnetization effect. Background Art
[0002] As an emerging technology in the field of non-destructive testing, weak magnetic stress detection technology supports non-contact, dynamic online detection compared with existing stress detection technologies (such as ultrasound, X-ray, coercive force, etc.), and has great application potential in the field of long-distance oil and gas pipeline stress internal detection technology. However, due to the complex environment of pipeline weak magnetic stress internal detection, weak magnetic signals and external magnetic fields can cause non-uniform magnetization of the pipeline wall. The magnetized pipeline wall will produce a demagnetization field, which interferes with signal detection, namely the demagnetization effect. Since the weak magnetic signal is weak and the magnetic permeability of the pipeline stress concentration area is enhanced, the demagnetization effect in the pipeline weak magnetic stress internal detection is more significant. The demagnetization effect can cause the intensity and characteristics of the weak magnetic signal to change, which affects the weak magnetic signal acquisition and identification. The demagnetization effect will generate a reverse magnetic field inside the ferromagnetic material, resulting in the detection of the stress concentration area inside the pipeline wall often missing detection or even undetectable. These factors seriously affect the detection efficiency of the pipeline weak magnetic stress internal detection technology. Therefore, a mathematical model for weak magnetic stress detection under the demagnetization effect is established, and then the detection characteristics of weak magnetic stress in pipelines under the demagnetization effect are quantitatively analyzed. It is particularly important to accurately model the weak magnetic stress detection, improve the detection accuracy of the system, and eliminate the demagnetization interference characteristics. Summary of the invention
[0003] In order to establish a mathematical model for the internal detection of weak magnetic stress in pipelines under the demagnetization effect, in order to realize the accurate quantitative analysis of the weak magnetic detection signal and the distribution characteristics of the demagnetization field in the pipeline stress detection environment, and then accurately determine the mathematical model of weak magnetic stress detection, clarify and eliminate the demagnetization interference characteristics. Based on the non-uniform magnetization of ferromagnetic media, the present invention introduces the demagnetization field as a secondary field source into the magnetomechanical calculation, establishes a weak magnetic stress detection model under the demagnetization effect, proposes an analytical analysis method for the relationship between the spatial weak magnetic signal and the spatial distribution of the demagnetization field, and establishes a finite element calculation and analysis model of the detection signal under the demagnetization effect according to the pipeline detection environment. A quantitative research method for the internal detection signal of weak magnetic stress in pipelines under the demagnetization effect is designed.
[0004] Step 1): Calculation of detection signal characteristics within weak magnetic stress
[0005] When ferromagnetic materials are damaged by stress, stress concentration areas will form at the damaged parts. Based on the solid electron energy band theory, it can be known that: in the stress concentration area, stress causes atoms to leave their equilibrium positions, resulting in the introduction of solid electrons into the complete ionic crystal, thereby causing the original periodic potential field to be locally distorted and the potential energy of the distorted area to increase. In order to maintain the principle of minimum energy, ferromagnetic materials use their own "molecular field" to rotate the magnetic domain vector, thereby generating magnetization intensity and externally manifesting magnetism. Weak magnetic stress detection technology evaluates the concentration of the pipeline by detecting this change in magnetic signals. Under stress, the magnetomechanical relationship of the pipeline wall is:
[0006]
[0007] Where M is the actual magnetization value, M an is the ideal magnetization, M s is the saturation magnetization, σ is the stress value; ε is the material stress coefficient, c is the reversible component coefficient, a is the molecular field parameter, and He is the equivalent magnetic field, which can be expressed as:
[0008]
[0009] Where F is the system energy, μ0 is the vacuum magnetic permeability, and λ is the magnetostriction coefficient of the ferromagnetic material. According to formula (2), the additional magnetic field H is required. e To know the value of the magnetostriction coefficient λ of the ferromagnetic material, we must know it. However, as a magnetic parameter of ferromagnetic materials, the magnetostriction coefficient is only related to the magnetic domain structure inside the ferromagnetic material, and it is not easy to obtain an accurate parameter value. Therefore, the empirical formula is used to approximate the simplified expression:
[0010]
[0011] Where γ i is the stress-determining parameter. As a simplification, when i = 2, an approximate estimate of the magnetostriction coefficient of the material is obtained:
[0012] λ≈γ1(σ)M 2 +γ2(σ)M 4 (4)
[0013] And γ(σ) can be expanded using Taylor series:
[0014]
[0015] In the formula, γ i (0) is when σ=0γ i The nth order derivative of . From equations (2), (3), (4), and (5), we can get:
[0016]
[0017] Where μ0 is the vacuum magnetic permeability. Substituting different stress values σ into equations (1) and (6), the corresponding magnetization intensity M of the ferromagnetic material can be determined. This is the magnetomechanical formula for ferromagnetic materials. However, this formula only calculates the magnetism of the material itself under stress, while our weak magnetic stress detection is to detect the spatial magnetic field distribution after the ferromagnetic material generates magnetism. For this reason, we introduce magnetomechanical calculations into Maxwell's equations to calculate the distribution of its spatial magnetic field. Under Maxwell's equations, the relationship between the magnetic field of ferromagnetic materials and the surrounding electric field can be expressed as:
[0018]
[0019] Where E is the electric field around the ferromagnetic material, χ is the meson magnetic susceptibility, σ0 is the meson conductivity, ε0 is the dielectric constant, l is the integral curve of the ferromagnetic material, S is the integral surface of the ferromagnetic material, is the rate of change of the electric field over time. In this equation, the corresponding relationship between the material magnetization intensity M and the surrounding electric field intensity E can be determined. From this formula, it can be seen that the generation of magnetization intensity M changes the original electric field E of the pipeline wall. The changing electric field excites the displacement current: Where I D That is the displacement current. Solving equation (1), equation (6), and equation (7) together, we can get the corresponding formula of displacement current and stress:
[0020]
[0021] Where V is the volume of the ferromagnetic material. A three-dimensional rectangular coordinate system is established with the center of the displacement current as the origin. Take any two current elements I with vectors R and -R on the displacement current. D dl, -I D dl, then the magnetic induction intensities dB1 and dB2 generated by the two current elements at any test point in space are:
[0022]
[0023]
[0024] Where r is the distance between the current source and the test point. After superposition of equation (9) and equation (10), the two current elements generate a weak magnetic signal strength dB0 at the test point:
[0025]
[0026] In the formula is the coordinate angle of the current element. The mathematical model of weak magnetic stress detection can be obtained by derivation of formula (11):
[0027]
[0028] Substituting this equation into different coordinate points (x, y, z), we can find the weak magnetic signal strength B0 generated by stress at any point in space. Therefore, we use the principle of electromagnetic coupling to introduce the previous pipeline magnetism calculation into Maxwell's equations, and then establish the magnetomechanical relationship of weak magnetic signals. However, in actual engineering, the pipeline wall will generate a demagnetization field due to its own demagnetization effect, which will interfere with signal detection. In order to clarify the interference characteristics of the demagnetization effect and improve the detection efficiency, we further add the demagnetization effect to the calculation of the weak magnetic stress detection mathematical model.
[0029] Step 2): Calculation of the detection signal characteristics of weak magnetic stress under demagnetization effect
[0030] In the weak magnetic stress internal inspection of pipelines, the magnetization phenomenon around the stress concentration area of the pipeline wall forms a demagnetization effect. Since non-uniform magnetic fields are difficult to calculate in a conventional way, in order to obtain the demagnetization field strength in weak magnetic stress detection, we must introduce other auxiliary quantities. For the static magnetic field generated by ferromagnetic materials, since there is no conduction current in the entire space, we can introduce the magnetic scalar potential to calculate the demagnetization field strength similar to the method of introducing potential in the electrostatic field.
[0031] Since the magnetic field is a spin-passive field, that is, a non-conservative field, it cannot be described by an electric potential like an electric field. However, we can see that under certain specific conditions, the integral of the magnetic field loop in this area is zero, so the magnetic scalar potential can be introduced. With the introduction of magnetic scalar potential and magnetic charge, some concepts in the electric field can be introduced into the magnetic field, as long as certain analogies are made. In the magnetic medium, if we want to find a magnetic field in the gap between the two poles of the electromagnet, we can introduce a potential in this area. Therefore, for the static magnetic field generated by ferromagnetic materials, since there is no conduction current in the entire space, we can also introduce the magnetic scalar potential to calculate the demagnetization field strength in a similar way to the method of introducing potential in the electrostatic field. In the magnetic charge model, the magnetic moment is p m The magnetic scalar potential formed by the magnetic dipole It can be expressed as:
[0032]
[0033] Where |rr′| is the vector from the magnetic dipole source point to the desired magnetic potential field point. Now consider a ferromagnetic body as composed of multiple magnetic dipoles, then the magnetic scalar potential of these magnetic dipoles at any point in space can be expressed as:
[0034]
[0035] Where M is the magnetization intensity of the ferromagnet. Using electrodynamics, the surface density of magnetic charge is: Magnetic charge density Then formula (14) can be further written as:
[0036]
[0037] In the static magnetic space formed by the ferromagnetic material, the positive and negative magnetic charges inside are neutralized, and the magnetic charges can be considered to be distributed on the surface, that is, there is only surface magnetic charge but no body magnetic charge. At this time, the demagnetization field B' is related to the magnetic scalar potential The corresponding relationship can be expressed as:
[0038]
[0039] Where B' is the demagnetization field strength, r' is the distance between the magnetic charge and the test point, r" is the magnetic charge radius, q m ″ is the total magnetic charge of the ferromagnetic material, which can be expressed as:
[0040]
[0041] Where V is the integrated volume of the ferromagnetic material, and S is the integrated area of the ferromagnetic material. By combining equations (15), (16), and (17), the demagnetization field intensity in weak magnetic stress detection can be obtained as:
[0042]
[0043] Where N is the demagnetization factor of the ferromagnetic material. Substituting this equation into different coordinate points (x, y, z) and magnetization intensity M, we can calculate the magnetic field intensity B′ generated by the ferromagnetic material with magnetization intensity M at any point in space. Therefore, we use the current distribution characteristics of the electrostatic field to introduce the magnetic scalar potential, and then complete the calculation of the demagnetization field in the weak magnetic stress detection of the pipeline. Combining equations (12) and (18) to obtain:
[0044]
[0045] Formula (19) is the mathematical model for weak magnetic stress detection under the demagnetization effect. Substituting this formula into the spatial position (x, y, z) and the magnetization intensity generated by the stress, the weak magnetic signal intensity under the demagnetization field effect can be calculated. Based on this mathematical model and formula (18), the interference characteristics of the demagnetization effect and the weak magnetic signal detection characteristics under the interference of the demagnetization effect can be quantitatively analyzed.
[0046] As a preferred solution, the present invention also includes an analytical algorithm modeling part for studying the demagnetization interference characteristics in weak magnetic stress internal detection. The method is: set a piece of pipeline wall material, take the stress damage area as the origin 0, and establish a three-dimensional Cartesian coordinate system. Set the angle between the line connecting any point on the bottom surface to the X-axis and the X-axis to φ.
[0047] As a preferred solution, the analytical algorithm can set the pipe wall material to be 450 mm long, 50 mm wide, 16 mm high, and 280 H / m in relative magnetic permeability. A transmission medium with a relative magnetic permeability of 1 H / m is distributed around the pipe wall material.
[0048] As a preferred solution, the present invention also includes a specific calculation analysis of the analytical model, including the following steps:
[0049] 1) Calculation of weak magnetic signal distribution characteristics without demagnetization: Take the X-axis as the scanning path, and the scanning range is -12mm*+12mm. Set the stress concentration range of the stress damage area to 50Mpa*300Mpa. Substitute into formula (12) to obtain the weak magnetic stress internal detection signal transmission characteristic diagram without demagnetization effect, and study the signal distribution characteristics.
[0050] 2) Calculation of demagnetization field distribution characteristics: Take the X-axis as the scanning path and the scanning range is -12mm-+12mm. Set the stress concentration range of the stress damage zone to 50Mpa-300Mpa. Substitute into formula (18) to obtain the demagnetization field distribution characteristic diagram in pipeline detection, and conduct a study on the demagnetization distribution characteristics.
[0051] 3) Calculation of weak magnetic signal distribution characteristics under demagnetization: Take the X-axis as the scanning path and the scanning range is -12mm-+12mm. Set the stress concentration range of the stress damage area to 30Mpa-300Mpa. Substitute into formula (19) to obtain the magnetic signal transfer characteristic diagram of the stress damage under demagnetization effect, and study the signal distribution characteristics under demagnetization effect.
[0052] As a preferred solution, the present invention also includes a modeling part of a finite element simulation model for studying and verifying the characteristics of the detection signal of the weak magnetic stress of the pipeline under the demagnetization effect. The modeling method is: using finite element simulation software to establish a pipeline model, set stress damage areas on the inner wall and outer wall of the pipe respectively, establish a three-dimensional coordinate system with the two stress damage areas as the origin, and map the magnetic space distribution of the detection signal.
[0053] As a preferred solution, the finite element model can be set to a model pipeline with a length of 100000 mm, a diameter of 1200 mm, a wall thickness of 16 mm, and an elastic modulus of 2*10 6 N / m -2 , Poisson's ratio PRXY is 0.3, and the relative magnetic permeability is 280H / m.
[0054] As a preferred solution, ANSYS is used as the finite element simulation model calculation software.
[0055] As a preferred solution, the present invention also includes a specific calculation analysis of a finite element simulation model, including the following steps:
[0056] 1) Calculation of the transmission characteristics of weak magnetic stress internal detection signals in transmission media: Calculation of the transmission characteristics of weak magnetic stress internal detection signals in transmission media: In order to obtain the transmission characteristics of the weak magnetic stress internal detection signals of stress damage in transmission media such as oil and gas, the acquisition rules of weak magnetic stress internal detection signals are clarified. We first set the stress concentration range of the stress damage zone on the inner wall of the pipeline to 200Mpa-400Mpa. Taking the stress damage zone on the inner wall of the pipeline as the origin, +80mm--80mm is taken as the scanning path of the internal detection detector along the positive and negative half axes of the X axis. The range of +2mm-+12mm (interval 2mm) along the positive half axis of the Z axis is taken as the lift-off value to calculate the magnetic induction intensity. The spatial distribution diagram of the magnetic signal of stress damage internal detection in the transmission medium is obtained. The tangential peak value and normal peak-valley value of the weak magnetic stress internal detection signal under different lift-off values in the spatial distribution diagram of the magnetic signal of stress damage internal detection in the transmission medium are extracted respectively, and the extracted values are exponentially fitted using the first-order exponential function f=A(1-*exp(-b*X)). The transfer characteristic diagram of the detection signal in the weak magnetic stress in the transmission medium is obtained, and then the detection signal in the transmission medium is analyzed and studied.
[0057] 2) Calculation of the transfer characteristics of the weak magnetic stress internal detection signal in the pipeline wall material: In order to obtain the transfer characteristics of the weak magnetic stress internal detection signal in the pipeline wall material, the internal detection characteristics of the stress damage zone on the outer wall of the pipeline are clarified. We first set the stress concentration range of the stress damage zone on the outer wall of the pipeline to 200Mpa-400Mpa. Taking the stress damage zone on the outer wall of the pipeline as the origin, +80mm--80mm is taken as the scanning path of the internal detector along the positive and negative semi-axis of the X-axis. Along the negative semi-axis of the Z-axis, the range of 2mm-12mm (interval 2mm) is taken as the transfer path of the weak magnetic stress internal detection signal in the damaged area in the pipeline wall material, and the magnetic induction intensity is calculated. The spatial magnetic distribution diagram of the weak magnetic stress internal detection signal of stress damage in the pipeline wall material is obtained, and the tangential peak value and normal peak-to-valley value of the detection magnetic signal in different transmission distances in the spatial magnetic distribution diagram of the weak magnetic stress internal detection signal of stress damage in the pipeline wall material are extracted respectively, and the transfer characteristic diagram of the weak magnetic stress internal detection signal in the pipeline wall material is obtained. Then the detection signal in the pipeline wall material is analyzed and studied.
[0058] (3) Calculation of excitation characteristics of weak magnetic stress internal detection signal: In order to obtain the excitation characteristics of the detection magnetic signal in pipeline stress internal detection, we further added an external magnetic field to the simulation model. The range of the external magnetic field is 50μt-75μt. The stress concentration level of the stress damage zone on the inner wall of the pipeline is set to 100Mpa. Taking the stress damage zone on the inner wall of the pipeline as the origin, +80mm--80mm is taken as the scanning path of the internal detector along the positive and negative half axes of the X-axis, and the lift-off value is set to 6mm to calculate the magnetic induction intensity. The characteristic diagram of the internal detection magnetic signal under the external magnetic field is obtained. The tangential peak value and the normal peak-to-valley value of the signal in the characteristic diagram of the internal detection magnetic signal under the external magnetic field are extracted respectively, and the BiHill curve is used to fit the excitation characteristic diagram of the internal detection magnetic signal. The detection signal characteristics under the external field are studied.
[0059] As a preferred solution, the present invention selects X80 pipe as experimental material, and designs a weak magnetic signal spatial transmission characteristic experiment under demagnetization effect and a weak magnetic signal characteristic experiment under external magnetic field.
[0060] As a preferred solution, the experimental material is an X80 pipe with a length of 10000mm, a diameter of 1219mm, and a wall thickness of 18.6mm. Four groups of cracks are made on the pipe, and the crack sizes are: No. 1 crack 50mm*2mm*3mm, No. 2 crack 50mm*2mm*2mm, No. 3 crack 50mm*1mm*2mm, No. 4 crack 50mm*1mm*1mm. The two ends of the pipe are closed with steel plates, and a "burst guardrail" is installed outside the pipe to prevent the pipe from bursting. Four cracks are made on the outer wall of the pipe. The pipe pressure is increased to 20.05MPa by a high-pressure liquid pressurization system, and the pressure is maintained for 5 minutes, and then the pressure is released. The pressure causes stress concentration at the crack, which in turn generates a weak magnetic signal. The degree of stress concentration increases with the increase of crack size.
[0061] As a preferred solution, four cracked pipe sections were cut from the X80 pipeline as experimental specimens. The size of the cut specimens is 450mm*50mm*18.6mm. Two cushion layers of non-ferromagnetic medium and ferromagnetic medium of different thicknesses were set at the cracks of the four specimens to simulate the two transmission environments of weak magnetic signals in the pipeline wall material and the transmission medium. The thickness of the ferromagnetic and non-ferromagnetic cushion layers ranges from 2mm to 12mm. A weak magnetic detection device (TSC-2M-8) was used to scan the crack tip along the length direction of the specimen to collect the weak magnetic signals of the tangential component and normal component of the specimen.
[0062] As a preferred solution, crack specimen No. 4 was selected as the experimental material, and the specimen was stretched using a tensile machine with a tensile force of 100 MPa. A metal strain gauge was attached to the crack of the specimen to collect stress values. An excitation coil was used to superimpose an external magnetic field on the specimen. A weak magnetic detection probe was attached to the inside of the excitation coil to collect tangential and normal weak magnetic signals of the specimen. The coil was connected to a current value of 1.5A-5.5A (interval 1A) to provide the specimen with external magnetic fields of different intensities. A forklift was used to drive the excitation coil up and down along the steel bar to achieve the effect of superimposing the external magnetic field and scanning detection. The weak magnetic signal strength under the geomagnetic field and different external magnetic fields, as well as the stress value at the crack were recorded respectively for experimental comparative analysis.
[0063] The invention has beneficial effects.
[0064] Based on the non-uniform magnetization of ferromagnetic media, the present invention introduces the demagnetization field as a secondary field source into the magnetomechanical calculation, and establishes a weak magnetic stress detection model under the demagnetization effect. Using this mathematical model, the interference characteristics of the demagnetization effect on the weak magnetic signal are analytically calculated, and the change law of the weak magnetic signal under different stresses and transmission distances is analyzed. We also established a finite element simulation model for internal detection of weak magnetic stress in pipelines under the demagnetization effect. The transmission law of weak magnetic signals in the transmission medium and the pipeline wall is calculated. The BiHill function is introduced to fit the external magnetic field excitation curve, and a new method for improving the detection signal analysis capability using an external excitation magnetic field is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods. The protection scope of the present invention is not limited to the following description.
[0066] Figure 1 Analytical model diagram.
[0067] Figure 2 a Calculation and analysis diagram of pipeline weak magnetic signal transmission characteristics.
[0068] Figure 2 b Calculation and analysis diagram of pipeline demagnetization field distribution characteristics.
[0069] Figure 2 c Calculation and analysis diagram of weak magnetic signal transmission characteristics under demagnetization effect.
[0070] Figure 3 a Pipeline simulation model diagram.
[0071] Figure 3 b Pipe wall simulation model diagram.
[0072] Figure 4 a Magnetic spatial distribution diagram of tangential weak magnetic signal in the transmission medium.
[0073] Figure 4b Magnetic spatial distribution of normal weak magnetic signal in transmission medium
[0074] Figure 5 a Magnetic transfer characteristics diagram of tangential weak magnetic signal in transmission medium.
[0075] Figure 5 b Magnetic transfer characteristics diagram of normal weak magnetic signal in transmission medium.
[0076] Figure 6 a Graph showing the tangential weak magnetic signal transmission characteristics in the transmission medium.
[0077] Figure 6 b Diagram of normal weak magnetic signal transmission characteristics in the transmission medium.
[0078] Figure 7 a Magnetomechanical curve of tangential weak magnetic signal.
[0079] Figure 7 b Magnetomechanical curve of normal weak magnetic signal.
[0080] Figure 8 a Magnetic spatial distribution diagram of tangential weak magnetic signal in pipeline wall material.
[0081] Figure 8 b Magnetic spatial distribution diagram of normal weak magnetic signal in pipeline wall material.
[0082] Fig. 9 a Tangential weak magnetic signal transmission characteristics in pipeline wall material
[0083] Fig. 9 b Normal weak magnetic signal transmission characteristics in pipeline wall material.
[0084] Fig.10 Equation coefficients chart.
[0085] Fig.11 a Characteristic diagram of tangential weak magnetic signal under external magnetic field.
[0086] Fig.11 b Characteristic diagram of normal weak magnetic signal under external magnetic field.
[0087] Fig.12 Weak magnetic signal excitation characteristic curve.
[0088] Fig.13 a. Pressurize the pipeline. Fig.13 b. Pipeline pressure relief system. Fig.14 a Pipeline interception material. Fig.14 b. Testing equipment. Fig.15 a Experimental diagram of weak magnetic signal transmission characteristics in ferromagnetic materials. Fig.15 b Experimental diagram of weak magnetic signal transmission characteristics in non-ferromagnetic materials. Fig.16 a Stretching and excitation system in the weak magnetic signal experiment under external magnetic field. Fig.16 b Control and display system in weak magnetic signal experiment under external magnetic field. Fig.17 a Experimental data diagram of tangential weak magnetic signal transmission characteristics in transmission medium. Fig.17 b Experimental data diagram of normal weak magnetic signal transmission characteristics in transmission medium. Fig.18 a Tangential weak magnetic signal magnetomechanical experimental data curve. Fig.18 b Normal weak magnetic signal magnetomechanical experimental data curve. Fig.19 a Experimental data diagram of tangential weak magnetic signal transmission characteristics in pipeline wall materials. Fig.19 b Experimental data of normal weak magnetic signal transmission characteristics in pipeline wall materials. Fig. 20 Equation coefficients chart. Fig.21 Mathematical model error contrast plot. Fig. 22 a Experimental data diagram of tangential weak magnetic signal characteristics under external magnetic field. Fig. 22 b Experimental data of normal weak magnetic signal characteristics under external magnetic field. Fig.23 Experimental data diagram of weak magnetic signal excitation characteristics. DETAILED DESCRIPTION
[0089] The present invention comprises the following steps:
[0090] Step 1): Calculation of detection signal characteristics within weak magnetic stress
[0091] When ferromagnetic materials are damaged by stress, stress concentration areas will form at the damaged parts. Based on the solid electron energy band theory, it can be known that: in the stress concentration area, stress causes atoms to leave their equilibrium positions, resulting in the introduction of solid electrons into the complete ionic crystal, thereby causing the original periodic potential field to be locally distorted and the potential energy of the distorted area to increase. In order to maintain the principle of minimum energy, ferromagnetic materials use their own "molecular field" to rotate the magnetic domain vector, thereby generating magnetization intensity and externally manifesting magnetism. Weak magnetic stress detection technology evaluates the concentration of the pipeline by detecting this change in magnetic signals. Under stress, the magnetomechanical relationship of the pipeline wall is:
[0092]
[0093] Where M is the actual magnetization value, M an is the ideal magnetization, M s is the saturation magnetization, σ is the stress value; ε is the material stress coefficient, c is the reversible component coefficient, a is the molecular field parameter, and He is the equivalent magnetic field, which can be expressed as:
[0094]
[0095] Where F is the system energy, μ0 is the vacuum magnetic permeability, σ is the applied stress, and λ is the magnetostriction coefficient of the ferromagnetic material. According to formula (2), the additional magnetic field H is required. e To know the value of the magnetostriction coefficient λ of the ferromagnetic material, we must know it. However, as a magnetic parameter of ferromagnetic materials, the magnetostriction coefficient is only related to the magnetic domain structure inside the ferromagnetic material, and it is not easy to obtain an accurate parameter value. Therefore, the empirical formula is used to approximate the simplified expression:
[0096]
[0097] Where γ i is the stress-determining parameter. As a simplification, when i = 2, an approximate estimate of the magnetostriction coefficient of the material is obtained:
[0098] λ≈γ1(σ)M 2 +γ2(σ)M 4 (4)
[0099] And γ(σ) can be expanded using Taylor series:
[0100]
[0101] In the formula, γ i (0) is when σ=0γ i The nth order derivative of . From equations (2), (3), (4), and (5), we can get:
[0102]
[0103] Where μ0 is the vacuum magnetic permeability. Substituting equations (1) and (6) into different stress values σ, the corresponding magnetization intensity M of the ferromagnetic material can be determined. This is the magnetomechanical formula for ferromagnetic materials. However, this formula only calculates the magnetism of the material itself under stress, while our weak magnetic stress detection is to detect the spatial magnetic field distribution after the ferromagnetic material generates magnetism. For this reason, we introduce magnetomechanical calculations into Maxwell's equations to calculate the distribution of its spatial magnetic field. Under Maxwell's equations, the relationship between the magnetic field of ferromagnetic materials and the surrounding electric field can be expressed as:
[0104]
[0105] Where E is the electric field around the ferromagnetic material, χ is the meson magnetic susceptibility, σ0 is the meson conductivity, ε0 is the dielectric constant, l is the integral curve of the ferromagnetic material, S is the integral surface of the ferromagnetic material, is the rate of change of the electric field over time. In this equation, the corresponding relationship between the material magnetization intensity M and the surrounding electric field intensity E can be determined. From this formula, it can be seen that the generation of magnetization intensity M changes the original electric field E of the pipeline wall. The changing electric field excites the displacement current: Where I D That is the displacement current. Solving equation (1), equation (6), and equation (7) together, we can get the corresponding formula of displacement current and stress:
[0106]
[0107] Where V is the volume of the ferromagnetic material. A three-dimensional rectangular coordinate system is established with the center of the displacement current as the origin. Take any two current elements I with vectors R and -R on the displacement current. D dl, -I D dl, then the magnetic induction intensities dB1 and dB2 generated by the two current elements at any test point in space are:
[0108]
[0109]
[0110] Where r is the distance between the current source and the test point. After superposition of equation (9) and equation (10), the two current elements generate a weak magnetic signal strength dB0 at the test point:
[0111]
[0112] In the formula is the coordinate angle of the current element. The mathematical model of weak magnetic stress detection can be obtained by derivation of formula (11):
[0113]
[0114] Substituting this equation into different coordinate points (x, y, z), we can find the weak magnetic signal strength B0 generated by stress at any point in space. Therefore, we use the principle of electromagnetic coupling to introduce the previous pipeline magnetism calculation into Maxwell's equations, and then establish the magnetomechanical relationship of weak magnetic signals. However, in actual engineering, the pipeline wall will generate a demagnetization field due to its own demagnetization effect, which will interfere with signal detection. In order to clarify the interference characteristics of the demagnetization effect and improve the detection efficiency, we further add the demagnetization effect to the calculation of the weak magnetic stress detection mathematical model.
[0115] Step 2): Calculation of the detection signal characteristics of weak magnetic stress under demagnetization effect
[0116] In the weak magnetic stress internal inspection of pipelines, the magnetization phenomenon around the stress concentration area of the pipeline wall forms a demagnetization effect. Since non-uniform magnetic fields are difficult to calculate in a conventional way, in order to obtain the demagnetization field strength in weak magnetic stress detection, we must introduce other auxiliary quantities. For the static magnetic field generated by ferromagnetic materials, since there is no conduction current in the entire space, we can introduce the magnetic scalar potential to calculate the demagnetization field strength similar to the method of introducing potential in the electrostatic field.
[0117] Since the magnetic field is a spin-passive field, that is, a non-conservative field, it cannot be described by an electric potential like an electric field. However, we can see that under certain specific conditions, the integral of the magnetic field loop in this area is zero, so the magnetic scalar potential can be introduced. With the introduction of magnetic scalar potential and magnetic charge, some concepts in the electric field can be introduced into the magnetic field, as long as certain analogies are made. In the magnetic medium, if we want to find a magnetic field in the gap between the two poles of the electromagnet, we can introduce a potential in this area. Therefore, for the static magnetic field generated by ferromagnetic materials, since there is no conduction current in the entire space, we can also introduce the magnetic scalar potential to calculate the demagnetization field strength in a similar way to the method of introducing potential in the electrostatic field. In the magnetic charge model, the magnetic moment is p m The magnetic scalar potential formed by the magnetic dipole It can be expressed as:
[0118]
[0119] Where |rr′| is the vector from the magnetic dipole source point to the desired magnetic potential field point. Now consider a ferromagnetic body as composed of multiple magnetic dipoles, then the magnetic scalar potential of these magnetic dipoles at any point in space can be expressed as:
[0120]
[0121] Where M is the magnetization intensity of the ferromagnet. Using electrodynamics, the surface density of magnetic charge is: Magnetic charge density Then formula (14) can be further written as:
[0122]
[0123] In the static magnetic space formed by the ferromagnetic material, the positive and negative magnetic charges inside are neutralized, and the magnetic charges can be considered to be distributed on the surface, that is, there is only surface magnetic charge but no body magnetic charge. At this time, the demagnetization field B' is related to the magnetic scalar potential The corresponding relationship can be expressed as:
[0124]
[0125] Where B' is the demagnetization field strength, r' is the distance between the magnetic charge and the test point, r" is the magnetic charge radius, q m″ is the total magnetic charge of the ferromagnetic material, which can be expressed as:
[0126]
[0127] Where V is the integrated volume of the ferromagnetic material, and S is the integrated area of the ferromagnetic material. By combining equations (15), (16), and (17), the demagnetization field intensity in weak magnetic stress detection can be obtained as:
[0128]
[0129] Where N is the demagnetization factor of ferromagnetic materials. Substituting this equation into different coordinate points (x, y, z) and magnetization intensity M, we can calculate the magnetic field intensity B′ generated by ferromagnetic materials with magnetization intensity M at any point in space. Therefore, we use the characteristics of electrostatic field current distribution, introduce magnetic scalar potential, and then complete the calculation of demagnetization field in pipeline weak magnetic stress internal detection. Combining equations (12) and (18) we get:
[0130]
[0131] Formula (19) is the mathematical model for weak magnetic stress detection under the demagnetization effect. Substituting this formula into the spatial position (x, y, z) and the magnetization intensity generated by the stress, the weak magnetic signal intensity under the demagnetization field effect can be calculated. Based on this mathematical model and formula (18), the interference characteristics of the demagnetization effect and the weak magnetic signal detection characteristics under the interference of the demagnetization effect can be quantitatively analyzed.
[0132] Depend on Figure 1 It can be seen that the present invention also includes an analytical algorithm modeling part for studying the demagnetization interference characteristics in weak magnetic stress internal detection. The method is: set a piece of pipeline wall material, take the stress damage area as the origin 0, and establish a three-dimensional Cartesian coordinate system. Set the angle between the line connecting any point on the bottom surface to the X-axis and the X-axis to φ.
[0133] The analytical algorithm can set the pipe wall material to be 450 mm long, 50 mm wide, 16 mm high, and 280 H / m in relative magnetic permeability. A transmission medium with a relative magnetic permeability of 1 H / m is distributed around the pipe wall material.
[0134] The present invention also includes a specific calculation analysis of the analytical model, including the following steps:
[0135] 1) Calculation of weak magnetic signal distribution characteristics without demagnetization: Take the X-axis as the scanning path, and the scanning range is -12mm*+12mm. Set the stress concentration range of the stress damage area to 50Mpa*300Mpa. Substitute into formula (12) to obtain the weak magnetic stress internal detection signal transmission characteristic diagram without demagnetization effect, and study the signal distribution characteristics.
[0136] Depend on Figure 2 (a) It can be seen that the weak magnetic signal decays exponentially with the increase of the transmission distance in the pipeline wall material and the transmission medium, and the signal strength is the same but in the opposite direction. The weak magnetic signal strength increases with the increase of stress.
[0137] 2) Calculation of demagnetization field distribution characteristics: Take the X-axis as the scanning path and the scanning range is -12mm-+12mm. Set the stress concentration range of the stress damage zone to 50Mpa-300Mpa. Substitute into formula (18) to obtain the demagnetization field distribution characteristic diagram in pipeline detection, and conduct a study on the demagnetization distribution characteristics.
[0138] Depend on Figure 2 (b) It can be seen that in the transmission medium, the demagnetization field decays exponentially with the increase of the transmission distance, and its transmission direction is the same as that of the weak magnetic signal. In the pipeline wall material, the demagnetization field first increases and then decays exponentially with the increase of the transmission distance, and its transmission direction is opposite to that of the weak magnetic signal. It can be seen that: in the transmission medium, the demagnetization effect produces a superimposed magnetic field, which interferes with signal detection and produces calculation errors. In the pipeline wall material, the demagnetization effect produces a reverse magnetic field, which causes the signal to decay faster and the signal strength to decrease. As the stress increases, the strength of the demagnetization field increases.
[0139] 3) Calculation of weak magnetic signal distribution characteristics under demagnetization: Take the X-axis as the scanning path and the scanning range is -12mm-+12mm. Set the stress concentration range of the stress damage area to 30Mpa-300Mpa. Substitute into formula (19) to obtain the magnetic signal transfer characteristic diagram of the stress damage under demagnetization effect, and study the signal distribution characteristics under demagnetization effect.
[0140] Depend on Figure 2 (c) It can be seen that under the demagnetization effect, the weak magnetic signal in the transmission medium still decays exponentially with the transmission distance, and the signal strength is enhanced compared with no demagnetization effect. Under the demagnetization effect, the weak magnetic signal in the pipeline wall material first fluctuates as a power function with the transmission distance, and then decays exponentially. Compared with no demagnetization effect, the signal strength decreases. As the stress increases, the strength of the weak magnetic signal increases.
[0141] Depend on Figure 3 It can be seen that the present invention also includes a modeling part of a finite element simulation model for studying and verifying the characteristics of the detection signal of the weak magnetic stress of the pipeline under the demagnetization effect. The modeling method is: using finite element simulation software to establish a pipeline model, set stress damage areas on the inner wall and outer wall of the pipe respectively, establish a three-dimensional coordinate system with the two stress damage areas as the origin, and map the magnetic space distribution of the detection signal.
[0142] The model pipeline can be set to have a length of 100000 mm, a diameter of 1200 mm, a wall thickness of 16 mm, and an elastic modulus of 2*10 6 N / m -2, Poisson's ratio PRXY is 0.3, and the relative magnetic permeability is 280H / m.
[0143] The ANSYS is used as the finite element simulation model calculation software.
[0144] The present invention also includes a specific calculation analysis of the finite element simulation model, including the following steps:
[0145] 1) Calculation of the transfer characteristics of the weak magnetic stress internal detection signal in the transmission medium: In order to obtain the transfer characteristics of the weak magnetic stress internal detection signal of stress damage in the transmission medium such as oil and gas, the collection rules of the internal detection signal are clarified. We first set the stress concentration range of the stress damage zone of the inner wall of the pipeline to 200Mpa-400Mpa. Taking the stress damage zone of the inner wall of the pipeline as the origin, +80mm--80mm is taken as the scanning path of the internal detection detector along the positive and negative half axes of the X axis. The range of +2mm-+12mm (interval 2mm) along the positive half axis of the Z axis is taken as the lift-off value to calculate the magnetic induction intensity. The spatial distribution diagram of the weak magnetic stress internal detection signal of stress damage in the transmission medium is obtained. The tangential peak value and normal peak-valley value of the internal detection magnetic signal under different lift-off values in the spatial distribution diagram of the weak magnetic stress internal detection signal of stress damage in the transmission medium are extracted respectively, and the extracted values are exponentially fitted with the first-order exponential function f=A(1-*exp(-b*X)). The transfer characteristic diagram of the weak magnetic stress internal detection signal in the transmission medium is obtained. Then the detection signal in the transmission medium is analyzed and studied.
[0146] Depend on Figure 4 , 5, 6, and 7 show that in the three areas of the weak magnetic transmission space, the lift-off value range of the sensitive area is 2mm-5mm, and the attenuation amplitude of the tangential and normal weak magnetic signals in this area is between 25% and 30%, indicating that the signal in this area fluctuates greatly with the lift-off value and is strongly affected by the jitter effect, so it is not suitable to set the lift-off value in this area. In addition, the detector probe is too close to the pipe wall, and it is easy for the probe to rub against the pipe wall and damage the probe. The lift-off value range of the linear area is 5mm-8mm, and the attenuation amplitude of the tangential and normal weak magnetic signals in this area is between 16% and 19%, indicating that the signal in this area fluctuates less with the lift-off value, so it is less affected by the jitter effect. In addition, the linear correlation coefficient in this area is the largest among the three areas, and the signal accuracy is the highest, making it most suitable for setting the lift-off value. The lift-off value range of the weak value zone is 8mm-12mm. The attenuation amplitude of the tangential and normal weak magnetic signals in this area is between 11%-14%. The attenuation amplitude is further reduced, but the weak magnetic signal intensity in this area is weak and the detection stress range is limited, so this area is not suitable for setting the lift-off value. The weak magnetic signal increases linearly with the increase of stress. When the lift-off value decreases from 12mm to 2mm, the slope of the tangential fitting curve increases from 72 to 122, and the slope of the normal fitting curve increases from 43 to 86, indicating that reducing the lift-off value can increase the slope of the signal magnetomechanical fitting curve, thereby increasing the magnetomechanical sensitivity of the weak magnetic signal.
[0147] 2) Calculation of the transmission characteristics of the weak magnetic stress detection signal in the pipeline wall material
[0148] In order to obtain the transmission characteristics of the weak magnetic stress internal detection signal in the pipeline wall material, the internal detection characteristics of the stress damage zone on the outer wall of the pipeline are clarified. We first set the stress concentration range of the stress damage zone on the outer wall of the pipeline to 200Mpa-400Mpa. Taking the stress damage zone on the outer wall of the pipeline as the origin, +80mm--80mm is taken along the positive and negative semi-axis of the X-axis as the scanning path of the internal detector. Along the negative semi-axis of the Z-axis, the range of 2mm-12mm (interval 2mm) is taken as the transmission path of the detection magnetic signal in the damage zone in the pipeline wall material, and the magnetic induction intensity is calculated. The spatial magnetic distribution diagram of the weak magnetic stress internal detection signal of stress damage in the pipeline wall material is obtained, and the tangential peak value and normal peak-valley value of the detection magnetic signal in different transmission distances in the spatial magnetic distribution diagram of the weak magnetic stress internal detection signal of stress damage in the pipeline wall material are extracted respectively, and the transmission characteristic diagram of the weak magnetic stress internal detection signal in the pipeline wall material is obtained. Then the detection signal in the pipeline wall material is analyzed and studied.
[0149] Depend on Figure 8 , 9It can be seen that in the pipeline wall material, the weak magnetic signal first fluctuates in a power function and then decays exponentially with the increase of the transmission distance. The greater the stress, the stronger the weak magnetic signal intensity. This characteristic does not change with the transmission distance. It can be seen that the greater the stress concentration on the outer wall of the pipeline, the stronger the anti-demagnetization interference of its weak magnetic signal in the pipeline wall material. The power function and exponential function are used to fit the extracted signal in sections, and the weak magnetic signal transmission equation inside the pipeline wall is obtained:
[0150]
[0151] In the formula, B is the strength of weak magnetic signal, D is the transmission distance of weak magnetic signal, a is the equation segmentation coefficient, which determines the boundary between power function and exponential function, A1, A2, A3 are fluctuation coefficients, which determine the degree of signal fluctuation, and b is the attenuation coefficient, which is inversely proportional to the signal attenuation speed.
[0152] Depend on Fig.10 It can be seen that as stress increases, the equation fluctuation coefficient increases and the attenuation coefficient decreases. This means that as stress increases, the signal fluctuation increases and the attenuation speed accelerates. The attenuation coefficient of the normal equation is greater than that of the tangential equation, which means that the normal signal decays slowly in the pipeline wall, has higher stability, and has a stronger ability to detect the stress concentration area on the outer wall of the pipeline.
[0153] (3) Calculation of excitation characteristics of weak magnetic stress detection signal
[0154] In order to obtain the excitation characteristics of the detection magnetic signal in the internal detection of pipeline stress, we further added an external magnetic field to the simulation model, and the range of the external magnetic field was 50μt-75μt. The stress concentration degree of the stress damage zone on the inner wall of the pipeline was set to 100Mpa. Taking the stress damage zone on the inner wall of the pipeline as the origin, +80mm--80mm was taken as the scanning path of the internal detector along the positive and negative half axes of the X-axis, and the lift-off value was set to 6mm to calculate the magnetic induction intensity. The characteristic diagram of the internal detection magnetic signal under the external magnetic field was obtained. The tangential peak value and the normal peak-to-valley value of the signal in the characteristic diagram of the weak magnetic stress internal detection signal under the external magnetic field were extracted respectively, and the BiHill function was introduced for fitting to obtain the excitation characteristic diagram of the internal detection magnetic signal. The detection signal characteristics under the external field were studied.
[0155] Depend on Fig.11 , 12 It can be seen that with the increase of the external magnetic field, the base value fluctuation of the weak magnetic signal increases and the signal attenuates. This is because the external magnetic field will enhance the demagnetization effect. Although the demagnetization effect in the transmission medium will increase the strength of the weak magnetic signal, it will also generate more interfering magnetic fields, which will eventually reduce the weak magnetic signal or even cover it. As the external magnetic field increases, the weak magnetic signal first increases and then decreases. The BiHill function signal fitting degree is as high as 99%. This fitting curve can be used to determine the optimal excitation magnetic field for weak magnetic stress detection and improve the signal detection capability.
[0156] Depend on Fig.13 It can be seen that the present invention selects X80 pipe as the experimental material, and designs the weak magnetic signal spatial transmission characteristic experiment and the weak magnetic signal characteristic experiment under the external magnetic field.
[0157] The experimental material is an X80 pipe with a length of 10000mm, a diameter of 1219mm, and a wall thickness of 18.6mm. Four groups of cracks are made on the pipe, and the crack sizes are: No. 1 crack 50mm*2mm*3mm, No. 2 crack 50mm*2mm*2mm, No. 3 crack 50mm*1mm*2mm, No. 4 crack 50mm*1mm*1mm. The two ends of the pipe are closed with steel plates, and a "burst protection fence" is installed outside the pipe to prevent the pipe from bursting. Four cracks are made on the outer wall of the pipe. The pipe pressure is increased to 20.05MPa using a high-pressure liquid pressurization system, maintained for 5 minutes, and then released. The pressure causes stress concentration at the crack, which in turn generates a weak magnetic signal. The degree of stress concentration increases with the increase of crack size.
[0158] Depend on Fig.14 , 15 It can be seen that four cracked pipe sections were cut from the X80 pipeline as experimental specimens. The size of the cut specimens is 450mm*50mm*18.6mm. Two types of cushion layers of non-ferromagnetic medium and ferromagnetic medium of different thicknesses were set at the cracks of the four specimens to simulate the two transmission environments of weak magnetic signals in the pipeline wall material and the transmission medium. The thickness of the ferromagnetic and non-ferromagnetic cushion layers varies from 2mm to 12mm. A weak magnetic detection device (TSC-2M-8) was used to scan the crack tip along the length direction of the specimen to collect weak magnetic signals of the tangential component and normal component of the specimen.
[0159] Depend on Fig.16 It can be seen that crack specimen No. 4 was selected as the experimental material, and the specimen was stretched using a tensile machine with a tensile force of 100MPa. A metal strain gauge was attached to the crack of the specimen to collect stress values. The specimen was superimposed with an external magnetic field using an excitation coil. The weak magnetic detection probe was attached to the inside of the excitation coil to collect the tangential and normal weak magnetic signals of the specimen. The coil was connected to a current value of 1.5A-5.5A (interval 1A) to provide the specimen with external magnetic fields of different intensities. The excitation coil was driven up and down along the steel bar by a forklift to achieve the effect of superimposing the external magnetic field and scanning detection. The geomagnetic field and the weak magnetic signal strength under different external magnetic fields, as well as the stress value at the crack were recorded respectively for experimental comparative analysis.
[0160] The specific steps of the experiment of the present invention are as follows:
[0161] Step 1): weak magnetic signal transmission characteristics in non-ferromagnetic medium (transmission medium): fit the tangential peak value and normal peak-to-peak value of the weak magnetic signal in the non-ferromagnetic medium to obtain the weak magnetic signal transmission characteristic diagram in the non-ferromagnetic medium. Fig.17It can be seen that the tangential peak point and normal zero point of the weak magnetic signal are both within the range of 68mm-75mm of the scanning path, which is the same as the position of the set stress concentration zone. With the increase of the lift-off value, the weak magnetic signal decays exponentially. In the sensitive areas of 2mm-5mm, 5mm-8mm, 8mm-12mm, and. The signal attenuation amplitudes in the tangential and normal directions are 30%-38%, 21%-28%, and 18%-25%, respectively, and the attenuation amplitude in the sensitive area is the largest. The linear correlation coefficients are 0.72-0.81, 0.91-0.96, and 0.80-0.86, respectively, and the linear correlation coefficient in the linear area is the largest. The average signal strength is 546nT-1342nT, 303nT-1037nT, and 137nT-631nT, and the average signal strength in the weak value area is the smallest. Fig.18 It can be seen that the weak magnetic signal increases linearly with the crack size, that is, the stress value. As the lift-off value decreases, the slope of the magnetomechanical curve increases. These are in good agreement with theoretical calculations.
[0162] Step 2): Weak magnetic signal transmission characteristics in ferromagnetic medium (pipeline wall material): Fit the tangential peak value and normal peak-to-peak value of the weak magnetic signal in the ferromagnetic medium to obtain the weak magnetic signal transmission characteristic diagram in the ferromagnetic medium. Fig.19 It can be seen that the intensity of weak magnetic signals in ferromagnetic media is smaller than that in non-ferromagnetic media. As the transmission distance increases, the weak magnetic signal first fluctuates as a power function and then decays exponentially. The greater the stress, the stronger the weak magnetic signal, and the transmission distance has no effect on this characteristic. The weak magnetic signal transmission equation inside the pipeline wall of formula (20) is used to fit the tangential peak value and the normal peak peak value, and the equation coefficients are shown in the table. Fig. 20 It can be seen that as stress increases, the equation fluctuation coefficient increases and the attenuation coefficient decreases. The attenuation coefficient of the normal equation is greater than that of the tangential equation. These are all in good agreement with theoretical calculations.
[0163] Step 3): Experiment on weak magnetic signal characteristics under external magnetic field: Using metal strain gauge and weak magnetic detection probe, the crack stress value under the geomagnetic field is measured to be 420Mpa, the tangential weak magnetic signal strength is 1100nT, and the normal weak magnetic signal strength is 1610nT. Substitute the stress values into equations (12) and (19) respectively to solve the weak magnetic signal strength of the weak magnetic stress detection mathematical model with and without demagnetization effect analysis. Compare and analyze the experimental data with the mathematical model data to obtain a comparison chart of the mathematical model error rate. By Fig.21 It can be seen that the calculation error rate of the weak magnetic stress detection model in the normal direction is 35.2%. After adding the demagnetization effect, the model error rate is 9.8%, and the error rate is reduced by 28.4%. The calculation error rate of the weak magnetic stress detection model in the normal direction is 35.4%. After adding the demagnetization effect analysis, the mathematical model error rate is 8.6%, and the error rate is reduced by 26.8%. After adding the demagnetization effect, the average error rate is reduced by 27.6%.
[0164] We use the weak signals collected under different external magnetic fields to extract the tangential peak value and normal peak-to-peak value of the weak magnetic signal, and use the BiHill function to fit the extracted peak value with the peak-to-peak value to produce the weak magnetic signal characteristic diagram under the external magnetic field. Fig. 22 , 23 It can be seen that the weak magnetic signal increases first and then decreases with the external magnetic field, and the BiHill function signal fitting degree reaches 97%. Using the fitting function, it can be seen that when the excitation coil is applied with a 3A current, the weak magnetic signal is most obvious and the detection characteristics are stronger.
[0165] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A quantitative research method for detecting internal signals of weak magnetic stress in pipelines under demagnetization effect, comprising the following steps: Step 1): Calculation of detection signal characteristics within weak magnetic stress When ferromagnetic materials are damaged by stress, stress concentration areas will form at the damaged parts. Based on the solid electron energy band theory, it can be known that in the stress concentration area, stress causes atoms to leave their equilibrium positions, resulting in the introduction of solid electrons into the complete ionic crystal, thereby causing the original periodic potential field to be locally distorted and the potential energy of the distorted area to increase. In order to maintain the principle of minimum energy, ferromagnetic materials use their own "molecular field" to rotate the magnetic domain vector, thereby generating magnetization intensity and externally manifesting magnetism. Weak magnetic stress detection technology evaluates the concentration of the pipeline by detecting this change in magnetic signals. Under stress, the magnetomechanical relationship of the pipeline wall is: Where M is the actual magnetization value, M an is the ideal magnetization, M s is the saturation magnetization, σ is the stress value; ε is the material stress coefficient, c is the reversible component coefficient, a is the molecular field parameter, and He is the equivalent magnetic field, which can be expressed as: Where F is the system energy, μ0 is the vacuum magnetic permeability, and λ is the magnetostriction coefficient of the ferromagnetic material. According to formula (2), the additional magnetic field H is required. e To know the value of the magnetostriction coefficient λ of the ferromagnetic material, we must know it. However, as a magnetic parameter of ferromagnetic materials, the magnetostriction coefficient is only related to the magnetic domain structure inside the ferromagnetic material, and it is not easy to obtain an accurate parameter value. Therefore, the empirical formula is used to approximate the simplified expression: Where γ i is the stress-determining parameter. As a simplification, when i = 2, an approximate estimate of the magnetostriction coefficient of the material is obtained: λ≈γ1(σ)M 2 +γ2(σ)M 4 (4) And γ(σ) can be expanded using Taylor series: In the formula, γ i (0) is when σ=0γ i The nth order derivative of . From equations (2), (3), (4), and (5), we can get: Where μ0 is the vacuum magnetic permeability, and γ1 and γ2 are stress-determined parameters. Substituting equations (1) and (6) with different stress values σ, the corresponding magnetization intensity M of the ferromagnetic material can be determined. This is the magnetomechanical formula for ferromagnetic materials. However, this formula only calculates the magnetism of the material itself under stress, while our weak magnetic stress detection is to detect the spatial magnetic field distribution after the ferromagnetic material generates magnetism. For this reason, we introduce magnetomechanical calculations into Maxwell's equations to calculate the distribution of its spatial magnetic field. Under Maxwell's equations, the relationship between the magnetic field of ferromagnetic materials and the surrounding electric field can be expressed as: Where E is the electric field around the ferromagnetic material, χ is the meson magnetic susceptibility, σ0 is the meson conductivity, ε0 is the dielectric constant, l is the integral curve of the ferromagnetic material, S is the integral surface of the ferromagnetic material, is the rate of change of the electric field over time. In this equation, the corresponding relationship between the material magnetization intensity M and the surrounding electric field intensity E can be determined. From this formula, it can be seen that the generation of magnetization intensity M changes the original electric field E of the pipeline wall. The changing electric field excites the displacement current: Where I D That is the displacement current. Solving equation (1), equation (6), and equation (7) together, we can get the corresponding formula of displacement current and stress: Where V is the volume of the ferromagnetic material. A three-dimensional rectangular coordinate system is established with the center of the displacement current as the origin. Take any two current elements I with vectors R and -R on the displacement current. D dl, -I D dl, then the magnetic induction intensities dB1 and dB2 generated by the two current elements at any test point in space are: Where r is the distance between the current source and the test point. After superposition of equation (9) and equation (10), the two current elements generate a weak magnetic signal strength dB0 at the test point: middle is the coordinate angle of the current element. The mathematical model of weak magnetic stress detection can be obtained by derivation of formula (11): Substituting this equation into different coordinate points (x, y, z), we can find the weak magnetic signal strength B0 generated by stress at any point in space. Therefore, we use the principle of electromagnetic coupling to introduce the previous pipeline magnetism calculation into Maxwell's equations, and then establish the magnetomechanical relationship of weak magnetic signals. However, in actual engineering, the pipeline wall will generate a demagnetization field due to its own demagnetization effect, which will interfere with signal detection. In order to clarify the interference characteristics of the demagnetization effect and improve the detection efficiency, we further add the demagnetization effect to the calculation of the weak magnetic stress detection mathematical model. Step 2): Calculation of the detection signal characteristics of weak magnetic stress under demagnetization effect In the weak magnetic stress internal inspection of pipelines, the magnetization phenomenon around the stress concentration area of the pipeline wall forms a demagnetization effect. Since non-uniform magnetic fields are difficult to calculate in a conventional way, in order to obtain the demagnetization field strength in weak magnetic stress detection, we must introduce other auxiliary quantities. For the static magnetic field generated by ferromagnetic materials, since there is no conduction current in the entire space, we can introduce the magnetic scalar potential to calculate the demagnetization field strength similar to the method of introducing potential in the electrostatic field. Since the magnetic field is a spin-passive field, that is, a non-conservative field, it cannot be described by an electric potential like an electric field. However, we can see that under certain specific conditions, the integral of the magnetic field loop in this area is zero, so the magnetic scalar potential can be introduced. With the introduction of magnetic scalar potential and magnetic charge, some concepts in the electric field can be introduced into the magnetic field, as long as certain analogies are made. In the magnetic medium, if we want to find a magnetic field in the gap between the two poles of the electromagnet, we can introduce a potential in this area. Therefore, for the static magnetic field generated by ferromagnetic materials, since there is no conduction current in the entire space, we can also introduce the magnetic scalar potential to calculate the demagnetization field strength in a similar way to the method of introducing potential in the electrostatic field. In the magnetic charge model, the magnetic moment is p m The magnetic scalar potential formed by the magnetic dipole It can be expressed as: Where rr' is the vector from the magnetic dipole source point to the desired magnetic potential field point. Now consider a ferromagnetic body as composed of multiple magnetic dipoles, then the magnetic scalar potential of these magnetic dipoles at any point in space can be expressed as: Where M is the magnetization intensity of the ferromagnet. Using electrodynamics, the surface density of magnetic charge is: Magnetic charge density Then formula (14) can be further written as: In the static magnetic space formed by the ferromagnetic material, the positive and negative magnetic charges inside are neutralized, and the magnetic charges can be considered to be distributed on the surface, that is, there is only surface magnetic charge but no body magnetic charge. At this time, the demagnetization field B' is related to the magnetic scalar potential The corresponding relationship can be expressed as: Where B' is the demagnetization field strength, r' is the distance between the magnetic charge and the test point, r" is the magnetic charge radius, q m ″ is the total magnetic charge of the ferromagnetic material, which can be expressed as: Where V is the integrated volume of the ferromagnetic material, and S is the integrated area of the ferromagnetic material. By combining equations (15), (16), and (17), the demagnetization field intensity in weak magnetic stress detection can be obtained as: Where N is the demagnetization factor of ferromagnetic materials. Substituting this equation into different coordinate points (x, y, z) and magnetization intensity M, we can calculate the magnetic field intensity B′ generated by ferromagnetic materials with magnetization intensity M at any point in space. Therefore, we use the current distribution characteristics of the electrostatic field, introduce the magnetic scalar potential, and then complete the calculation of the demagnetization field in the weak magnetic stress detection of the pipeline. Combining equations (12) and (18) to obtain: Formula (19) is the mathematical model for weak magnetic stress detection under the demagnetization effect. Substituting this formula into the spatial position (x, y, z) and the magnetization intensity generated by the stress, the weak magnetic signal intensity under the demagnetization field effect can be calculated. Based on this mathematical model and formula (18), the interference characteristics of the demagnetization effect and the weak magnetic signal detection characteristics under the interference of the demagnetization effect can be quantitatively analyzed. The present invention also includes an analytical algorithm modeling part for studying the demagnetization interference characteristics in the weak magnetic stress internal detection of pipelines. The method is: set a piece of pipeline wall material, take the stress damage area as the origin 0, and establish a three-dimensional Cartesian coordinate system. Set the angle between the line connecting any point on the bottom surface to the X-axis and the X-axis to φ. The present invention also includes a modeling part of a finite element simulation model for studying and verifying the characteristics of a detection signal within a pipeline weak magnetic stress under a demagnetization effect. The modeling method is: use finite element simulation software to establish a pipeline model, set stress damage zones on the inner wall and outer wall of the pipe respectively, establish a three-dimensional coordinate system with the two stress damage zones as the origin, and map the magnetic space distribution of the detection signal.
2. According to the method for quantitatively studying the internal detection signal of weak magnetic stress in pipelines under demagnetization effect in claim 1, it is characterized in that The analytical algorithm can set the length of the pipe wall material to 450mm, the width to 50mm, the height to 16mm, and the relative magnetic permeability to 280H / m. A transmission medium with a relative magnetic permeability of 1H / m is distributed around this pipe wall material.
3. According to the method for quantitatively studying the internal detection signal of weak magnetic stress in pipeline under demagnetization effect in claim 1, it is characterized in that The finite element simulation model uses ANSYS as the finite element simulation model calculation software. The model can be set to a pipeline length of 100000mm, a diameter of 1200mm, a wall thickness of 16mm, and an elastic modulus of 2*10 6 N / m -2 , Poisson's ratio PRXY is 0.3, and the relative magnetic permeability is 280H / m.