Optical laminate, transparent display including same, and method of manufacturing same

By using silicon-based adhesives and optically transparent adhesive materials to form a functional layer between the metal film and the glass substrate, the problems of adhesion and heat resistance are solved, surface roughness and haze are reduced, and the transparent display is improved visibility and environmental adaptability.

CN118736973APending Publication Date: 2024-10-01DONGWOO FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410378053.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-29
Filing Date
2024-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When using metal films on glass substrates, the existing technology suffers from insufficient adhesion, poor heat resistance and poor reliability in high temperature and high humidity environments, resulting in increased surface roughness and haze, affecting the visibility of the transparent display.

Method used

Silicone adhesive is used as the adhesive layer, and optically transparent adhesive resin and adhesive are combined to form a functional layer to enhance adhesion and chemical resistance, reduce surface roughness, and reduce haze.

Benefits of technology

It improves the adhesion between the glass substrate and the metal layer, enhances chemical resistance to etching liquids and reliability in high temperature and high humidity environments, reduces surface roughness and haze, and improves the visibility of transparent displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118736973A_ABST
    Figure CN118736973A_ABST
Patent Text Reader

Abstract

The present invention relates to an optical laminate and a method for manufacturing the same, the optical laminate comprising: a glass substrate; an adhesive layer formed on one surface of the glass substrate; a metal layer pattern formed on one surface of the adhesive layer; and a functional layer provided on a portion on one surface of the adhesive layer where the metal layer pattern is not formed, the adhesive layer including a silicon-based adhesive, and the functional layer including one or more selected from the group consisting of an optically clear adhesive resin (OCR) and an optically clear adhesive (OCA).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical laminate, a transparent display including the same and a method for manufacturing the same. Background Art

[0002] Recently, in the display market, the demand for large-area display devices has been increasing due to technological advances. Advanced electronic circuits and display businesses such as Micro-LED (micro light-emitting diode) and Mini-LED (mini light-emitting diode) that can control the contrast and brightness per unit area are also being developed. In addition, photolithography methods for producing electronic devices that meet large area sizes, high resolution, and contrast quality are being studied.

[0003] Korean Patent Publication No. 10-2019-0003025 also discloses a circuit board and a method for manufacturing the same using a patterning process for a metal layer on top of a glass substrate.

[0004] However, conventionally, various methods such as electroplating or vapor deposition of metal thin films have been used as methods for realizing low-resistance metal wiring on glass substrates, but each of these methods has limitations due to the increase in the area of ​​displays.

[0005] In order to overcome such limitations, attempts have recently been made to develop a technology that patterns the metal thin film by using a photolithography method after bonding the metal thin film to a glass substrate.

[0006] However, the problem with this method of bonding a metal thin film to a glass substrate is that not only is the adhesion between the metal thin film and the glass substrate insufficient, but also the lower adhesive layer exposed after the metal layer is patterned is damaged by contact with a metal etching solution.

[0007] Furthermore, when used in electronic devices such as transparent displays that are exposed to the external environment for a long time, heat resistance and reliability in high temperature and high humidity environments are very important. However, in the case of acrylic adhesives or epoxy adhesives used in existing metal films, there is a problem of insufficient heat resistance and reliability in high temperature and high humidity environments.

[0008] To solve this problem, when a metal film is bonded to a glass substrate using a silicone adhesive, the surface shape of the originally laminated metal will remain on the surface of the adhesive that is peeled off after the metal film is patterned, thereby creating roughness on the surface. Accordingly, when applied to a display, light is scattered on the surface of the adhesive layer where the metal film pattern is not formed, increasing the haze and causing a problem of reduced visibility.

[0009] Therefore, there is a need to develop an optical laminate and a transparent display having improved visibility in addition to adhesion to a glass substrate, chemical resistance to a metal layer etching solution, heat resistance, and reliability under a high-temperature and high-humidity environment.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Korean Patent Publication No. 10-2019-0003025 Summary of the invention

[0013] Technical issues

[0014] An object of the present invention is to provide an optical laminate having excellent adhesion to a glass substrate and excellent chemical resistance to etching liquid, heat resistance and reliability, that is, an optical laminate and a transparent display having improved visibility by reducing the haze of the surface.

[0015] Another object of the present invention is to provide a method for producing the optical layered body and the transparent display.

[0016] Technical Solution

[0017] The present invention relates to an optical laminate, comprising: a glass substrate; an adhesive layer formed on one surface of the glass substrate; a metal layer pattern formed on one surface of the adhesive layer; and a functional layer, which is arranged on a portion of one surface of the adhesive layer where the metal layer pattern is not formed, wherein the adhesive layer comprises a silicon-based adhesive, and the functional layer comprises one or more selected from an optically transparent adhesive resin (OCR) and an optically transparent adhesive (OCA).

[0018] According to the present invention, in a first aspect, the functional layer may be provided on the metal layer pattern.

[0019] According to the present invention, in the second aspect, the thickness of the metal layer may be 3 μm to 120 μm.

[0020] According to the present invention, in a third aspect, the metal layer may include one or more selected from the group consisting of copper (Cu), aluminum (Al), nickel (Ni), chromium (Cr), silver (Ag), iron (Fe), gold (Au), cobalt (Co), titanium (Ti) and tungsten (W).

[0021] According to the present invention, in the fourth aspect, the thickness of the adhesive layer may be 5 μm to 50 μm.

[0022] According to the present invention, in the fifth aspect, no separate component may be included between the metal layer and the adhesive layer.

[0023] According to the present invention, in a sixth aspect, the adhesion between the adhesive layer and the glass substrate may be 5B or more.

[0024] The present invention relates to a transparent display comprising the optical laminate and a light emitting diode (LED).

[0025] According to the present invention in a seventh aspect, a transparent cover may be further included in the outermost portion corresponding to the glass substrate of the optical laminate.

[0026] According to the present invention, in an eighth aspect, the transparent cover may be one or more selected from glass, wired glass, colored glass, magic mirror, and holographic glass.

[0027] According to the present invention, in a ninth aspect, when the transparent cover is glass, it may further include at least one selected from wired glass, colored glass, magic mirror, and holographic glass.

[0028] In addition, the present invention relates to a method for manufacturing an optical laminate, comprising: a step of preparing a metal film, wherein the metal film includes a silicon-based adhesive layer formed on one side of a metal layer, and includes a first protective film provided on one side of the silicon-based adhesive layer and a second protective film provided on the other side of the metal layer; a step of peeling off the first protective film of the metal film; a step of bonding the metal film in a manner such that an adhesive layer is arranged on one side of a glass substrate; a step of peeling off the second protective film of the metal film; a step of patterning the metal layer to form a metal layer pattern; and a step of forming a functional layer in a portion where the metal layer pattern is not formed, the functional layer including one or more selected from an optically transparent adhesive resin (OCR) and an optically transparent adhesive (OCA).

[0029] According to the present invention, in the tenth aspect, the step of forming the metal layer pattern may include: the step of forming a photoresist pattern on one side of the metal layer; the step of etching the exposed area of ​​the metal layer through the photoresist pattern; and the step of stripping the photoresist pattern.

[0030] According to the present invention in the eleventh aspect, the lower adhesive layer may not be damaged in the etching step.

[0031] Effects of the Invention

[0032] According to the optical layered body and the transparent display of the present invention, the effect of improving visibility can be obtained by reducing the surface roughness and the haze. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 : are diagrams showing optical layered bodies according to one or more embodiments of the present invention.

[0034] Figure 2 is a diagram illustrating a transparent display according to one or more embodiments of the present invention.

[0035] Figure 3 It is a diagram showing a method for manufacturing a transparent display according to an embodiment of the present invention.

[0036] Figure 4 The method for manufacturing a transparent display according to an example of the present invention is a diagram showing a step of forming a functional layer on a metal layer pattern on which light emitting diodes 70 (LEDs) are formed.

[0037] Reference numerals

[0038] 10: metal layer, 20: adhesive layer, 30: protective film, 40: glass substrate, 50: photoresist pattern, 60: functional layer, 70: light emitting diode. DETAILED DESCRIPTION

[0039] The present invention relates to an optical laminate having an adhesive layer including a silicon-based adhesive, a transparent display and a method for manufacturing the same. Since the adhesive surface peeled off after patterning of a metal film includes a functional layer, the surface roughness is reduced and the haze is reduced, thereby having the effect of improving visibility.

[0040] In more detail, the present invention relates to an optical laminate, a transparent display and a method for manufacturing the same, wherein the optical laminate comprises: a glass substrate; an adhesive layer formed on one side of the glass substrate; a metal layer pattern formed on one side of the adhesive layer; and a functional layer provided on a portion of one side of the adhesive layer where the metal layer pattern is not formed, the adhesive layer comprising a silicon-based adhesive, and the functional layer comprising one or more selected from an optically transparent adhesive resin (OCR) and an optically transparent adhesive (OCA).

[0041] The embodiments of the present invention are described in more detail below with reference to the accompanying drawings. However, the following drawings attached to this specification illustrate preferred embodiments of the present invention and are used together with the above-mentioned invention content to further understand the role of the technical concept of the present invention, so the present invention should not be limited to the matters recorded in such drawings for interpretation.

[0042] The terms used in this specification are used to describe the embodiments and are not intended to limit the present invention. In this specification, unless otherwise stated in the context, the singular form also includes the plural form. For example, the "protective film" used in this specification may refer to at least one of the first protective film and the second protective film.

[0043] The terms "comprises" and / or "comprising" used in this specification are used to mean that they do not exclude the existence or addition of one or more other constituent elements, steps, actions and / or elements other than the mentioned constituent elements, steps, actions and / or elements. Throughout the specification, the same reference numerals refer to the same constituent elements.

[0044] "Below", "bottom", "lower part", "above", "top", "upper part" and the like as spatially relative terms can be used as shown in the figure to facilitate the description of the correlation between one element or constituent element and other elements or constituent elements. Spatially relative terms should be understood as terms that include different directions of elements when in use or operation in addition to the directions shown in the drawings. For example, when the elements shown in the figure are turned over, an element described as "below" or "lower part" of another element can also be placed "above" another element. Therefore, the exemplary term "below" can include both upper and lower directions. Elements can also be oriented in other directions, and accordingly, spatially relative terms can also be interpreted based on the orientation.

[0045] The term “substantially” as used in this specification may be interpreted as including not only being physically identical or identical but also being within a range of error in measurement or manufacturing process, for example, an error range of less than 0.1%.

[0046] <Optical laminate and transparent display>

[0047] Figure 1 1 is a diagram showing an optical laminate according to one or more embodiments of the present invention. Figure 2 is a diagram illustrating a transparent display according to one or more embodiments of the present invention.

[0048] Reference Figure 1 and Figure 2 , the optical laminate of one or more embodiments of the present invention may include a glass substrate 40, an adhesive layer 20, a metal layer 10 pattern, and a functional layer 60. In addition, the transparent display of the present invention may include the optical laminate, and a light emitting diode (LED). In addition, the transparent display may further include a transparent cover, and may further include a transparent cover (not shown) in the outermost contour corresponding to the glass substrate of the optical laminate. The transparent cover may be one or more selected from glass, wired glass, colored glass, magic mirror, and holographic glass. In addition, according to the present invention, when the transparent cover is glass, it may also include one or more selected from wired glass, colored glass, magic mirror, and holographic glass.

[0049] The glass substrate 40 is not particularly limited as long as it does not hinder the optical properties of the optical laminate, and can include, for example, oxide glass such as silicate glass, borate glass, phosphate glass, etc. In this case, there are advantages in that thermal shrinkage does not occur in subsequent processes, etc., and a predetermined hardness can be given to the optical laminate.

[0050] In one or more embodiments, the thickness of the glass substrate 40 may be 0.5 mm to 20 mm. When the thickness of the glass substrate 40 satisfies the range, the hardness is excellent and thinness can be achieved, and deformation or cracks of the metal layer 10 can be prevented. Specifically, when it is less than 0.5 mm, it may be difficult to protect the metal layer 10 or other laminated components from external impact, and when it exceeds 20 mm, it may be disadvantageous in thinness or lightness.

[0051] In one or more embodiments, the glass substrate 40 may have a single-layer or multi-layer structure. For example, the glass substrate 40 may have a single-layer structure formed by a single glass substrate, but is not necessarily limited thereto, and may also have a multi-layer structure having a plurality of glass substrates stacked.

[0052] In one embodiment, the optical laminate may include an adhesive layer 20 on one surface of the glass substrate 40 .

[0053] The adhesive layer 20 can be made of an adhesive layer composition including a silicon-based adhesive. The adhesive layer composition of the present invention includes a silicon-based additive and a solvent, and may further include an additive. Specifically, in the case of an adhesive layer formed using an existing acrylic adhesive or epoxy adhesive, there is a problem of insufficient adhesion to the glass substrate, or the adhesive layer is damaged by an etching solution used to etch a metal layer formed on the upper part of the adhesive layer. Furthermore, as in the case of a transparent display, when used for a product mainly used outdoors, there is a problem of decreased adhesion between the adhesive layer and the glass substrate or yellowing of the adhesive layer, which becomes a cause of product failure.

[0054] In order to solve this problem, the inventors of the present invention have proposed the present invention with a view to achieving excellent adhesion to the glass substrate when the adhesive layer 20 includes a silicon-based adhesive, and also having excellent chemical resistance to etching liquid, heat resistance, and reliability in a high-temperature and high-humidity environment.

[0055] The silicon-based adhesive may be one or more of a silicon-based compound and a siloxane compound.

[0056] The use of the silicon compound is not particularly limited as long as it is a compound including a silicon (Si) atom. In addition, the siloxane compound can use a compound including a siloxane bond of a Si-O bond without limitation. More specifically, in one example of the present invention, the silicon compound and the siloxane compound can be one or more of trimethylated silica, vinyl terminated polydimethylsiloxane, hexamethyl di siloxane, trisiloxane, and tetrakis (trimethylsilyloxy) silane.

[0057] In particular, preferably, the silicone adhesive of the present invention is contained in 40% to 60% relative to the total weight of the adhesive layer composition. Thus, the silicone adhesive of the present invention can be diluted and added at a concentration lower than that of conventional adhesives, and accordingly, when the adhesive layer of the present invention is bonded to a metal layer or a glass substrate, the adhesion to the metal layer or the glass substrate can be maximized, thereby having the advantage of achieving bonding without additional treatment such as UV curing of the adhesive layer.

[0058] The solvent is not particularly limited as long as it can dilute the silicon-based adhesive, and can be, for example, toluene, xylene, PGME, and / or PGMEA. From the perspective of the stability of the adhesive coating thickness under the metal layer, it is preferred that the solvent of the present invention is contained in an amount of 40% to 55% relative to the total weight of the adhesive layer composition.

[0059] The additive may be one or more of an anchoring agent, a cross linker, and a catalyst.

[0060] The anchoring agent is added to increase the bonding strength with the metal layer when the adhesive layer is applied, and can prevent the adhesive layer from separating from the metal layer. Generally, there is no special restriction on the material used as the anchoring agent, but it is preferred that the material does not deform under heat at 200°C or below.

[0061] The crosslinking agent is a substance added for chemical bonding between the components of the adhesive layer composition, and is preferably a product that does not undergo thermal deformation at 200° C. or below.

[0062] The catalyst is a component added for curing the adhesive layer composition, and helps the adhesive layer composition to transform from a liquid phase to a solid phase. As specific examples, platinum catalysts, palladium catalysts, and / or osmium catalysts can be used.

[0063] From the aspect of stability of adhesive force, it is preferred that the additive of the present invention is contained in an amount of 0.1 to 10% relative to the total weight of the adhesive layer composition.

[0064] The adhesive layer 20 of the present invention may be formed by heating and curing the adhesive layer composition at a temperature of 100° C. to 180° C.

[0065] The thickness of the adhesive layer 20 may be 5 μm to 50 μm, preferably 5 μm to 30 μm, preferably 5 μm to 25 μm. When the thickness of the adhesive layer 20 is less than 5 μm, sufficient adhesion with other components cannot be maintained, and when the thickness exceeds 50 μm, it may be disadvantageous in increasing the thickness of the product.

[0066] In one embodiment, the adhesive layer 20 may not include a separate component, such as an intermediate layer or a protective layer, at the contact interface with the metal layer 10. Specifically, in the case of using a conventional acrylic adhesive or epoxy adhesive to form the adhesive layer, there are problems such as damage to the adhesive layer due to the etching solution used to form the etching on the adhesive layer that does not reach the metal layer, such as in the case of an adhesive layer formed by an epoxy adhesive, the non-transparency of the adhesive layer increases when in contact with the etching solution. Therefore, in the conventional optical laminate, in order to prevent the etching solution from causing damage to the adhesive layer, a component of an intermediate layer or a protective layer is separately included between the adhesive layer and the metal layer. However, when a separate component is included in this way, not only does the processability decrease and the manufacturing cost increase due to the increase in the manufacturing process, but there is also a problem of disadvantage in the production of the film. However, in the present invention, as described above, by using a silicone adhesive with excellent chemical resistance to the etching solution to form the adhesive layer, damage to the adhesive due to the etching solution does not occur, and therefore, a component of an intermediate layer or a protective layer that was previously provided to protect the adhesive is not separately included. By not including a separate member, it is advantageous not only in terms of improving processability but also in terms of reducing manufacturing costs, and further advantageous in terms of thinning the film.

[0067] In one embodiment, the adhesion between the adhesive layer 20 and the glass substrate 40 may be 5B or more. As described above, the adhesive layer 20 includes a silicon-based adhesive, and thus has a characteristic of excellent adhesion between the adhesive layer 20 and the glass substrate 40 .

[0068] In one embodiment, the adhesion strength of the adhesive layer 20 to the glass substrate 40 can be evaluated by measuring the standard ISO 2409: Standard Test Methods for Measuring Adhesion by Tape Test.

[0069] The metal layer 10 can be used as an electrode in an electronic device such as a display device including the optical laminate.

[0070] There is no particular limitation on the metal layer 10 as long as it is conductive. For example, it may include one or more selected from the group consisting of copper (Cu), aluminum (Al), nickel (Ni), chromium (Cr), silver (Ag), iron (Fe), gold (Au), cobalt (Co), titanium (Ti) and tungsten (W).

[0071] The metal layer 10 can be formed by a well-known metal thin film process, for example, by preparing and attaching a metal thin film, or by using at least one of electroless deposition, electrodeposition, sputtering, thermal evaporation, and electron beam evaporation, but is not limited thereto.

[0072] The thickness of the metal layer 10 may be 3 μm to 120 μm, preferably 3 μm to 110 μm, and more preferably 18 μm to 105 μm. When the thickness of the metal layer 10 is less than 3 μm, it may not be easy to form a uniform film or pattern, and when the thickness exceeds 120 μm, there may be a problem that it cannot be applied to electronic devices with thin film structures.

[0073] The functional layer 60 is formed on the portion of the adhesive layer 20 where the metal layer 10 pattern is not formed, that is, formed on the adhesive layer 20 exposed by etching the metal layer when the metal layer 10 pattern is formed. The functional layer 60 can be formed by filling Figure 1 The portion where the metal layer 10 pattern is not formed is formed, more specifically, as shown Figure 2 As shown, it may be formed in a form connected to a portion of the adhesive layer 20 where the metal layer 10 is not formed and stacked on the metal layer pattern 10 where the light emitting diode 70 (LED) is formed.

[0074] On the other hand, as described above, the metal layer 10 is stacked on one surface of the adhesive layer 20 of the present invention, and the metal layer 10 may have a surface roughness (Rz) of 0.1 to 20 μm.

[0075] At this time, since the adhesive layer 20 includes a silicon-based adhesive layer, the surface morphology of the metal layer 10 is directly reflected in the adhesive layer 20. Therefore, when the metal layer 10 is peeled off after patterning, the surface of the adhesive layer 20 exposed by etching the metal layer generates concavities and convexities derived from the metal layer having a certain surface roughness, thereby causing light scattering when applied to a transparent display, resulting in a problem of increased haze.

[0076] Therefore, the functional layer 60 is provided at the portion of the adhesive layer 20 where the metal layer 10 pattern is not formed to prevent the surface unevenness of the adhesive layer 20 from occurring, thereby preventing scattering and reducing haze to improve visibility.

[0077] In this regard, the surface roughness (Rz) of the functional layer 60 may be 5.0 μm or less. When the surface roughness (Rz) exceeds 5.0 μm, scattering occurs, haze increases, and there is a problem of visual blurring.

[0078] The functional layer 60 can be formed of one or more selected from acrylic resins such as ethylene vinyl acetate (EVA) in the form of optically clear adhesive resin (OCR) or optically clear adhesive (OCA), polyethylene compounds such as polyvinyl butyral (PVB), and silicone resins, and can preferably be formed of acrylic resin or silicone resin.

[0079] The functional layer 60 stacked on the metal layer 10 may have a thickness of 1 μm to 3 mm.

[0080] As the light emitting diode (LED) 70 of the present invention, a known light emitting diode (LED) can be applied without limitation.

[0081] <Method for producing optical laminate and transparent display>

[0082] A method for manufacturing an optical laminate according to one embodiment of the present invention includes: a step of preparing a metal film, wherein the metal film includes a silicon-based adhesive layer 20 formed on one side of a metal layer 10, and includes a first protective film 30-1 provided on one side of the silicon-based adhesive layer 20, and a second protective film 30-2 provided on the other side of the metal layer 10; a step of peeling off the first protective film 30-1 of the metal film; a step of bonding the metal film in a manner such that the adhesive layer 20 is arranged on one side of a glass substrate 40; a step of peeling off the second protective film 30-2 of the metal film; a step of patterning the metal layer 10 to form a metal layer pattern; and a step of forming a functional layer 60 on a portion where the pattern of the metal layer 10 is not formed.

[0083] In addition, the manufacturing method of the transparent display of the present invention further includes the step of mounting a light emitting diode 70 (LED) in the manufacturing method of the optical laminate. Specifically, before the step of forming the functional layer 60, the step of mounting the light emitting diode 70 (LED) on the metal layer pattern may be included. In addition, after the step of mounting the light emitting diode 70 (LED) on the metal layer pattern, the step of covering one side of the optical laminate of the present invention, that is, the opposite side of the glass substrate 40, with a glass cover (not shown) may be included.

[0084] Figure 3 and Figure 4 It is a diagram showing a method for manufacturing a transparent display according to an embodiment of the present invention.

[0085] Specifically, in the step of peeling off the first protective film provided on the metal thin film, the first protective film 30 - 1 disposed on the lower surface of the adhesive layer 20 of the metal thin film may be peeled off.

[0086] The protective film 30 can be provided to protect the surface of the metal layer 10 and / or the adhesive layer 20 from external damage. For example, it can be provided in the form of a second protective film 30-2 formed on one surface of the metal layer 10 to protect the surface of the adhesive layer 20 and to protect the first protective film 30-1 formed on one surface of the adhesive layer 20 and the surface of the metal layer 10.

[0087] In one embodiment, the protective film can be used as Figure 2 Although a single-layer structure is shown, the present invention is not limited thereto and may be a multi-layer structure in which one or more protective films are continuously stacked.

[0088] In one embodiment, as for the protective film 30 , a second protective film 30 - 2 and a first protective film 30 - 1 may be laminated on one surface of the metal layer 10 and the adhesive layer 20 respectively by using a laminator.

[0089] The protective film 30 is not particularly limited as long as it is used to protect the surface of the metal layer 10 and / or the adhesive layer 20. For example, it can include a material selected from polyethylene terephthalate (PET), polyethylene isophthalate (PEI), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), diacetyl cellulose, triacetyl cellulose (TAC), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polymethyl acrylate (PMA), polyimide (PI), polymethyl methacrylate (PMMA), polyethyl acrylate (PEA), polyethyl methacrylate (PEMA), and cyclic olefin polymer (cyclic olefin polymer). In terms of availability and processing convenience, polyethylene terephthalate (PET), triacetylcellulose (TAC), polycarbonate (PC), polyimide (PI), and cyclic olefin polymer (COP) can be preferably used.

[0090] The thickness of the protective film 30 is not particularly limited, and may be, for example, 10 μm to 200 μm.

[0091] On the other hand, although the above-mentioned metal film takes the metal film having the protective film 30 on one side of the metal layer 10 and the adhesive layer 20 respectively as an example, it is not limited to this. For example, it may also include only one of the protective film formed on one side of the metal layer and the protective film formed on one side of the adhesive layer.

[0092] In the step of peeling off the first protective film provided on the metal thin film, the first protective film 30 - 1 disposed on the lower surface of the adhesive layer 20 of the metal thin film may be peeled off.

[0093] The first protective film 30 - 1 may be peeled off as appropriate within a range that does not hinder the purpose of the present invention, and a method used in a conventional process of peeling off a release film may be used.

[0094] In the step of bonding the metal thin film so as to arrange the adhesive layer on one surface of the glass substrate, the surface of the adhesive layer 20 exposed to the outside by peeling off the first protective film 30 - 1 may be bonded to one surface of the glass substrate 40 .

[0095] The bonding of the adhesive layer 20 and the glass substrate 40 may be appropriately performed within a range that does not hinder the purpose of the present invention. For example, the bonding may be performed using a laminator or the like.

[0096] In the step of peeling off the second protective film provided on the metal thin film, the second protective film 30 - 2 disposed on the upper surface of the metal layer 10 of the metal thin film may be peeled off.

[0097] The peeling of the second protective film 30 - 2 may be performed by substantially the same method as the peeling of the first protective film 30 - 1 .

[0098] On the other hand, although the above Figure 3 The method for manufacturing a transparent display is described by taking a method for manufacturing a transparent display using a metal thin film as an example, but is not limited thereto.

[0099] For example, in another embodiment of the present invention, when the metal thin film does not include the second protective film 30 - 2 , the step of peeling off the second protective film provided on the metal thin film may be omitted.

[0100] The steps of forming a pattern of the metal layer 10 of an optical stack according to an embodiment of the present invention may include: forming a photoresist pattern 50 on one side of the metal layer 10; etching the exposed area of ​​the metal layer 10 through the photoresist pattern; and stripping the photoresist pattern.

[0101] Specifically, the step of forming a photoresist pattern 50 on one side of the metal layer 10 may include: a process of coating a composition for forming a photoresist pattern on the metal layer 10 by spin coating, slit coating, inkjet printing, etc., and a process of drying and heat treating the coated composition for forming a photoresist pattern to form a photoresist film, and a process of forming the photoresist pattern 50 by selectively exposing and developing the photoresist film to dissolve and remove the photoresist film corresponding to the exposed area or the non-exposed area.

[0102] The step of forming the photoresist pattern 50 can be performed by a known method, and the details are omitted here.

[0103] The step of etching the exposed region of the metal layer 10 through the photoresist pattern 50 is not particularly limited, and may be performed by a dry etching process or a wet etching process.

[0104] In one embodiment, the wet etching process can be performed using an etching solution including at least one selected from the group consisting of nitric acid, phosphoric acid, and acetic acid. As described above, the bonding layer 20 is characterized in that it includes a silicon-based adhesive and has excellent chemical resistance to an etching solution including at least one selected from the group consisting of nitric acid, phosphoric acid, and acetic acid. Therefore, when the etching process is performed by wet etching based on an etching solution including at least one selected from the group consisting of nitric acid, phosphoric acid, and acetic acid, not only is the etching performance of the metal layer 10 excellent, but even if the bonding layer 20 located at the bottom of the metal layer 10 is exposed to the etching solution, it is possible to achieve that no damage (physical and chemical damage and white turbidity phenomenon) to the bonding layer 20 occurs.

[0105] The dry etching process or the wet etching process may be performed by a known method, and the details are omitted here.

[0106] The step of stripping the photoresist pattern may be performed by immersing the substrate having the resist pattern 50 formed thereon in a resist stripping solution, or by spraying the stripping solution onto the substrate, etc. In this case, a physical treatment such as ultrasonic irradiation, contact with a rotating or swinging brush, etc. may also be used.

[0107] In one embodiment, as the resist stripping condition, the temperature can be about 15°C to 100°C, preferably 30°C to 70°C, and the immersion or spraying time is preferably about 1 minute to 20 minutes, but is not limited thereto and can be appropriately modified according to user needs.

[0108] In one embodiment, after the resist stripping solution treatment, a cleaning process may be further performed to remove the stripping solution remaining on the substrate. The cleaning process may be performed in the same manner as the stripping process described above, except that water or isopropyl alcohol is used instead of the stripping solution.

[0109] In the present invention, the step of mounting the light emitting diode 70 (LED) on the metal layer pattern may use a method of performing surface mounting (SMT: Surface Mount Technology) on the device by soldering, but is not limited thereto.

[0110] More specifically, the patterned metal layer 10 of the metal film substrate may further include a solder layer (not shown), through which the light emitting diodes 70 (LEDs) may be mounted. The configuration interval or density of the light emitting diodes (LEDs) is not particularly limited, but may be configured in a grid form. In this case, the upper, lower, left, and right spacings may be 1 to 50 mm, and the spacings of the plurality of light emitting diodes (LEDs) may be the same or different from each other. When light emitting diodes (LEDs) are formed on the metal film substrate of the present invention, it has the advantage of being a transparent display capable of emitting and playing images on a substrate having transparency.

[0111] After the step of mounting the light emitting diode 70 (LED) on the metal layer pattern, a step of covering one side of the optical laminate of the present invention, that is, the side opposite to the glass substrate 40, with a glass cover (not shown) may be further included.

[0112] More specifically, in the step of forming the functional layer 60 described later, when an optically transparent adhesive resin (OCR) is applied, after the step of mounting the light emitting diode 70 (LED) on the metal layer pattern and before the step of forming the functional layer 60, after covering the opposite side of the glass substrate 40 of the optical laminate of the present invention with a transparent cover, the optically transparent adhesive resin (OCR) can be injected between the transparent cover and the glass substrate 40.

[0113] In addition, in the step of forming the functional layer 60 described later, when an optically transparent adhesive (OCA) is applied, after the step of mounting the light emitting diode 70 (LED) on the metal layer pattern, the functional layer 60 can be formed by attaching the optically transparent adhesive (OCA) and covering the opposite side of the glass substrate 40 of the optical laminate of the present invention with a transparent cover (not shown).

[0114] Specifically, Figure 4 A method for manufacturing a transparent display according to an example of the present invention is a diagram showing a step of forming a functional layer on a metal layer pattern having a light emitting diode 70 (LED) formed thereon. In one embodiment of the present invention, the step of forming the functional layer 60 may be formed of one or more selected from acrylic resins such as ethylene-vinyl acetate (EVA) in the form of optically transparent adhesive resins (OCR) or optically transparent adhesives (OCA), polyethylene compounds such as polyvinyl butyral (PVB), and silicone resins, and preferably, may be formed of acrylic resins or silicone resins.

[0115] The method of forming the functional layer 60 is not particularly limited, but may be manufactured by coating and curing the optically clear adhesive resin (OCR), and may be manufactured by cutting and attaching an optically clear adhesive (OCA) in accordance with a position to be attached.

[0116] The coating can be performed by a known method, generally by a knife coater, a roll coater, a calender coater, a comma coater, etc. In addition, depending on the coating thickness or the viscosity of the resin, it can also be performed using a gravure coater, a rod coater, etc.

[0117] The optical laminate of the present invention exhibits the above-mentioned characteristics, and therefore has the advantage that it can be suitable for use in display devices that require a large area and low resistance, and has excellent heat resistance and reliability in high temperature and high humidity environments, and is particularly suitable for use in devices such as transparent displays that may be exposed to the external environment for a long time.

[0118] Hereinafter, experimental examples including specific embodiments and comparative examples will be presented to help understand the present invention, but these are only illustrative of the present invention and do not limit the scope of the appended claims. It is obvious to those skilled in the art that various changes and modifications can be made to the embodiments within the scope of the scope of the present invention and the technical idea, and it is obvious that such changes and modifications also fall within the scope of the appended claims. In addition, unless otherwise stated, the "%" and "parts" indicating the content hereinafter are based on weight.

[0119] Examples and Comparative Examples: Preparation of Optical Laminated Body

[0120] Example 1

[0121] 4 kg of 99% toluene was added to 10 kg of silicone adhesive (96-083 Silicone Adhesive Kit, DOW; solid content 70%) to prepare a composition containing 50% silicone adhesive, which was then stirred with a stirrer (5 horsepower) and further mixed with 0.5 g of an anchoring agent (SYL-OFF TM SL-9250, DOW), 0.8 g crosslinker (SYL-OFF TM 7678, DOW), and 1 gram of platinum catalyst 1 g to prepare an adhesive layer composition.

[0122] Then, the adhesive layer composition was coated on one side of a 35 μm thick copper metal substrate (surface roughness (Rz) 9.0 μm) using a gravure coating method, and then cured at 150° C. for 2 minutes to produce a metal thin film having a 10 μm thick silicon-based adhesive layer formed on one side of the metal substrate.

[0123] After that, the adhesive layer of the metal thin film was disposed on one surface of a glass substrate having a thickness of 2 mm, and then the metal thin film was bonded by a sheet-to-sheet method to laminate a metal layer.

[0124] Afterwards, if Figure 3 As shown, the metal layer pattern is formed by patterning the metal layer using a photolithography method.

[0125] By forming a portion of the adhesive layer where the metal layer pattern is not formed Figure 1 An optically clear adhesive (CEF 8319-6, 3M) was filled and coated on the metal layer to form a functional layer, thereby manufacturing the optical laminate of Example 1. At this time, the thickness of the portion laminated on the metal layer of the functional layer was 1500 μm.

[0126] Example 2

[0127] In addition to replacing optically clear adhesives (CEF 8319-6, 3M), optically clear resins (Scotchcast TM An optical laminate was produced in the same manner as in Example 1 except for Resin 8, 3M).

[0128] Example 3

[0129] An optical laminate was produced in the same manner as in Example 1 except that a copper metal substrate having a thickness of 35 μm (surface roughness (Rz) 0.9 μm) was used.

[0130] Comparative Example 1

[0131] An optical layered body was produced in the same manner as in Example 1 except that the functionality was not formed.

[0132] Comparative Example 2

[0133] An optical layered body was produced in the same manner as in Example 3 except that the functional layer was not formed.

[0134] Experimental example

[0135] (1) Transmittance and haze evaluation

[0136] The transmittance and haze of the optical laminates of Examples and Comparative Examples were measured using a haze meter HM-150N (Murakami). The results are shown in Table 1 below.

[0137]

Table 1

[0138] distinguish Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Transmittance (%) 80.9 80.1 88.4 78.6 85.3 Haze 17.5 16.9 4.1 79.1 12.5

[0139] With reference to Table 1 above, it can be confirmed that the optical layered bodies of Examples including the functional layer of the present invention have excellent transmittance and significantly low haze compared to Comparative Examples not including the functional layer of the present invention.

[0140] That is, when comparing the optical laminates of Examples 1, 2 and Comparative Example 1 using metal substrates having the same surface roughness (Rz), and comparing the optical laminates of Example 3 and Comparative Example 2, it can be confirmed that the optical laminate of the embodiment including the functional layer of the present invention has excellent transmittance and significantly lower haze than the comparative example not including the functional layer of the present invention.

Claims

1. An optical laminate, It is characterized in that include: Glass substrate; an adhesive layer formed on one side of the glass substrate; a metal layer pattern formed on one side of the adhesive layer; as well as a functional layer provided on a portion of the adhesive layer on which the metal layer pattern is not formed, The adhesive layer includes a silicon-based adhesive, The functional layer includes at least one selected from an optically transparent adhesive resin and an optically transparent adhesive.

2. The optical layered body according to claim 1, It is characterized in that The functional layer is disposed on the metal layer pattern.

3. The optical layered body according to claim 1, It is characterized in that The thickness of the metal layer is 3 μm to 120 μm.

4. The optical layered body according to claim 1, It is characterized in that The metal layer includes at least one selected from the group consisting of copper, aluminum, nickel, chromium, silver, iron, gold, cobalt, titanium, and tungsten.

5. The optical layered body according to claim 1, It is characterized in that The adhesive layer has a thickness of 5 μm to 50 μm.

6. The optical layered body according to claim 1, It is characterized in that No separate components are included between the metal layer and the adhesive layer.

7. The optical laminate according to claim 1, It is characterized in that The adhesion between the adhesive layer and the glass substrate is 5B or more.

8. A transparent display, It is characterized in that include: The optical laminate according to any one of claims 1 to 7; as well as Light Emitting Diode.

9. The transparent display according to claim 8, It is characterized in that The optical laminate further includes a transparent cover at the outermost portion corresponding to the glass substrate.

10. The transparent display according to claim 9, It is characterized in that The transparent cover is one or more selected from glass, wired glass, colored glass, magic mirror, and holographic glass.

11. The transparent display according to claim 10, It is characterized in that When the transparent cover is glass, it also includes at least one selected from wired glass, colored glass, magic mirror, and holographic glass.

12. A method for producing an optical laminate, It is characterized in that include: The step of preparing a metal thin film, wherein the metal thin film includes a silicon-based adhesive layer formed on one side of a metal layer, and includes a first protective film provided on one side of the silicon-based adhesive layer and a second protective film provided on the other side of the metal layer; A step of peeling off the first protective film of the metal film; The step of bonding the metal thin film by disposing an adhesive layer on one surface of the glass substrate; A step of peeling off the second protective film of the metal film; a step of patterning the metal layer to form a metal layer pattern; and forming a functional layer on a portion where the metal layer pattern is not formed, The functional layer includes at least one selected from an optically transparent adhesive resin and an optically transparent adhesive.

13. The method for producing an optical layered body according to claim 12, It is characterized in that The step of forming the metal layer pattern comprises: forming a photoresist pattern on one side of the metal layer; The step of etching the exposed areas of the metal layer through the photoresist pattern; and The step of stripping the photoresist pattern.