Copper paste suitable for PCB hole filling and preparation method thereof

By using copper nanoparticles with ligands on the surface and copper paste with organic carriers, the problems of high cost and serious pollution in the PCB hole filling process are solved, high-precision conduction and stability are achieved, and the performance and performance of HDI products are improved. Production quality.

CN118737520APending Publication Date: 2024-10-01ENOVATE3D (HANGZHOU) TECH DEV CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310338284.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing PCB hole filling process has high operating costs, serious environmental pollution, prone to filling defects such as holes and depressions, and is difficult to achieve high-precision dimensional requirements.

Method used

A copper slurry composed of copper nanoparticles with ligands on the surface and an organic carrier is used to prepare copper nanoparticles through a liquid phase reduction method, and latent curing agents and acidic antioxidants are added to the organic carrier to form a one-component system. Improve stability and antioxidant properties.

Benefits of technology

It achieves low-cost, low-pollution, high-precision hole filling, with a conduction yield of ≥95%, and maintains stability in a 0-5°C environment, avoiding problems with holes and cracks, and improving the performance and production quality of HDI products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737520A_ABST
    Figure CN118737520A_ABST
Patent Text Reader

Abstract

The invention relates to the field of conductive paste, in particular to copper paste suitable for PCB hole filling and a preparation method thereof.The copper paste is composed of copper nanoparticles with ligands on the surfaces and an organic carrier; wherein the organic carrier comprises matrix resin, a latent curing agent, a diluent and an organic carrier auxiliary agent; the organic vehicle auxiliary agent comprises an antioxidant with acidity. The production cost of the prepared copper paste is far lower than that of silver paste in the same application scene, the operation process is simple, the working environment is good, the copper paste can replace a high-pollution acid copper electroplating process in production in the printing electronic industry, the replacement value is extremely high, and meanwhile, by adjusting the variety and proportion of organic carriers and selecting different volatile solvents for compounding and adding, the production cost is greatly reduced. Good morphology can be maintained, and no pore and cracking defect problems exist in inner and outer areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of conductive paste, and in particular to a copper paste suitable for PCB hole filling and a preparation method thereof. Background Art

[0002] As electronic technology develops towards lightweight, high-speed and miniaturization, the demand for higher-density multi-layer interconnection of printed circuit boards (PCBs) continues to increase. High-density interconnection (HDI) can greatly improve the transmission rate of PCBs and is the basic technology achieved by Anylayer. Its key preparation process is any-layer interconnection and micro-poration processing between layers. After the micropores are opened, metallization treatment or filling with conductive materials is required to achieve conduction between layers. At present, there are mainly three types of interconnection processes in mass production or development: any-layer: electroplating, printing and copper bump processes.

[0003] 1) For the electroplating hole filling process, it is generally achieved through acid copper electroplating. The existing patent CN101873770A publicly describes a circuit board copper electroplating hole plugging process. The micro-holes that need to be plugged through the through-holes are filled with copper plating technology through the electroplating principle. However, the operating cost of the technical equipment is high, and there are serious environmental pollution problems, which does not meet the needs of green development. If the longitudinal depth of the board is large, it is often impossible to evenly deposit single copper, which can easily cause product quality defects.

[0004] 2) For traditional printing processes, conductive paste is usually directly scraped onto the PCB board, which requires low product precision. With the technical trend of small apertures and high aspect ratio holes, the difficulty of printing has increased significantly, and filling defects such as voids and depressions and curing cracks are prone to occur. Patent CN 113025230 A discloses a thermally conductive and conductive copper paste, a preparation method and its application, which uses copper powder with a particle size D50 of 5μm to 30μm to prepare copper paste for printing PCB plug holes. Due to its large particle size, there are problems such as waste of raw materials and insufficient hole filling during the printing process, which limits the improvement of product quality. Another patent CN114334221A discloses a plug hole copper paste and its preparation method, and a printed circuit board. The particle size of the original copper paste used is sub-micron, and the application is described as a 5mm aperture size scenario, which is not as good as the precision size requirements of HDI below 100 microns.

[0005] 3) For the copper bump process, more fine-sized products can be produced, but the technology is difficult and mass production cannot be achieved yet.

[0006] In addition, due to the poor conductivity of pure copper paste after sintering, it is generally used in products with high heat dissipation requirements. For products that require conductivity, the industry mostly uses silver paste or silver-coated copper paste for preparation. For example, patent CN 102262918 B describes a silver paste for hole filling for printed circuit boards and its preparation method, and patent WO 2021 / 220711 A1 publicly introduces a conductive composition used in hole filling scenarios. Both use silver-coated particles or pure silver particles with an average particle size (D50) greater than 1μm as metal fillers to prepare conductive paste. Due to the high cost of silver raw materials, the complex preparation process of silver-coated particles, and the serious technical monopoly, it is difficult to use it as a preferred choice.

[0007] In summary, developing a conductive copper paste suitable for precision hole filling to break through the limitations of high-precision PCB production technology is of great significance to the development of the precision electronics industry. Summary of the invention

[0008] The present invention aims to overcome the defects of the prior art printed circuit board (PCB) hole filling process, such as high operating cost, serious environmental pollution, easy to produce voids and depressions, etc., and provides a copper paste suitable for PCB hole filling and a preparation method thereof to overcome the above problems.

[0009] To achieve the above-mentioned purpose, the present invention is implemented by the following technical solutions: In a first aspect, the present invention first provides a copper paste suitable for PCB hole filling. It is composed of copper nanoparticles with ligands on the surface and an organic carrier; wherein: The particle size of the copper nanoparticles is ≤1 μm; The organic carrier comprises a main resin, a latent curing agent, a diluent and an organic carrier auxiliary agent; The organic carrier auxiliary agent includes an acidic antioxidant.

[0010] Different from the prior art solution of directly using commercial copper powder dispersed in an organic medium, the copper slurry of the present invention uses surface-liganded copper nanoparticles prepared by a liquid phase reduction method, which can improve its own antioxidant properties on the one hand; on the other hand, it can increase its dispersion performance in the carrier, achieving excellent stability and uniformity.

[0011] The preparation method of the copper nanoparticles with ligands on the surface can be prepared by referring to the company's existing patent "A low-temperature copper paste suitable for high-precision 3D printing and its preparation method and application" (CN115188523A). The nano copper particles prepared by this method have a particle size of less than 1μm, so they are suitable for filling high-precision through holes and blind holes with an aperture of ≤100μm, and the conduction yield is ≥95%, which can solve the low-precision problem of traditional printing process products to a certain extent, and is expected to achieve the improvement of HDI product performance and production quality.

[0012] In addition to the copper nanoparticles used, the core point of the present application lies in the selection of the type of organic carrier in the copper paste.

[0013] Regarding the organic carrier, the main body of the organic carrier in this application is the main resin, which has a low thermal expansion coefficient. This is because the printed circuit board will generate heat during actual use. Selecting a resin with a low thermal expansion coefficient can avoid defects such as volume expansion, local cracking, and holes caused by heat during use, thereby improving the temperature resistance and service life of the product.

[0014] In order to allow the main resin to solidify smoothly, the present application also adds a certain amount of curing agent to the organic carrier. However, the inventors of the present application found that after the curing agent is added to the main resin, a reaction will occur immediately, causing the viscosity of the system to gradually increase over time. In order to overcome this problem in the prior art, the curing agent is usually added before use to form a two-component system. However, this system is prone to problems such as cumbersome glue preparation and unstable slurry viscosity. Therefore, the present application deliberately chooses to use a latent curing agent, which is pre-configured into a single-component system, which can greatly extend the storage period of the system, thereby effectively overcoming the above problems.

[0015] The inventors found in the test that copper nanoparticles will form a layer of copper oxide film on the surface after oxidation, which greatly improves the resistivity of copper paste after sintering. Therefore, the present invention adds an acidic antioxidant to the organic carrier additive to prevent the oxidation of copper nanoparticles. At the same time, the inventors also found that the type of antioxidant has a relatively obvious effect on the long-term antioxidant effect of copper paste. When the reducing ability of the selected reducing agent is too strong, for example, hydrazine hydrate is selected as a reducing agent. In theory, its antioxidant effect is better, but its antioxidant persistence is weak, and the reduction effect of oxidized copper oxide is poor. In the present invention, an acidic antioxidant is deliberately selected, which can first react with copper oxide to form copper ions, and at the same time, through its reducing ability, copper ions can be reduced to copper metal, solving the problem that conventional reducing agents are difficult to reduce copper oxide. At the same time, due to its reducing ability at a medium level, the duration of its reduction is longer, which can effectively improve the storage stability and process adaptability of the slurry.

[0016] Preferably, the content of the organic carrier accounts for 5-25% of the total mass of the copper paste, and the content of the copper nanoparticles accounts for ≥75% of the total mass of the copper paste.

[0017] Preferably, the organic carrier comprises, by weight, 100 parts of a main resin, 1 to 10 parts of a latent curing agent, 10 to 30 parts of a diluent, and 10 to 40 parts of an auxiliary agent.

[0018] Preferably, in the present application, the solid content of the copper slurry is controlled to be not less than 75% through the ratio design of the carrier components, so that the mass loss of the copper slurry before and after sintering is ≤5%, which can effectively avoid cracks, holes and depressions caused by excessive shrinkage.

[0019] Preferably, the main resin is a thermosetting resin with a thermal expansion coefficient of ≤100 ppm / K.

[0020] More preferably, the main resin is a thermosetting resin with a thermal expansion coefficient of ≤50 ppm / K.

[0021] Preferably, the main resin includes any one or more combinations of bisphenol A epoxy resin, bisphenol F epoxy resin, and alicyclic epoxy resin.

[0022] More preferably, the bisphenol A epoxy resin may be selected from products with brands such as Epikote 828, Epikote 827, and YD-128.

[0023] More preferably, the bisphenol F epoxy resin may be selected from products with a brand name such as NPEF-170.

[0024] More preferably, the alicyclic epoxy resin may be selected from products with a brand name such as TDE-85.

[0025] Preferably, the latent curing agent includes any one or more combinations of dicyandiamide and its derivatives, organic acid hydrazides, and boron trichloride amine complexes.

[0026] More preferably, the dicyandiamide and its derivatives can be selected from the brands UR200, UR300, UR500 (Alzchem, Germany); 2844 and other products.

[0027] Preferably, the organic acid hydrazide can be selected from products such as succinic acid dihydrazide, adipic acid dihydrazide, isophthalic acid dihydrazide and the like.

[0028] Preferably, the boron trichloride amine complex can be selected from products with brands such as ACCELERATOR DY 9577, BF-piperidine, Anchor 1115, etc.

[0029] Preferably, the diluent is a mono / diepoxy reactive diluent or an inactive diluent having a boiling point of 80-120°C.

[0030] The applicant has found that the boiling point of the diluent has a great influence on the morphology of the copper slurry after sintering. When the boiling point of the diluent used is low, its volatility is high, resulting in poor storage stability of the slurry and local agglomeration problems due to the volatilization of the diluent; at the same time, during the curing process, the diluent quickly vaporizes, resulting in poor density of the copper slurry after curing, thereby affecting its conduction effect. When the boiling point of the diluent used is high, a part of the diluent still remains in the cured system after curing, resulting in problems such as bubbles in the pores after sintering. Therefore, the present invention selects an organic solvent with a medium boiling point (boiling point of 80-120°C) as a diluent component, which, on the one hand, improves the dispersion performance of the particles in the organic phase; on the other hand, it is adapted to the "drying-curing" production process, so that it can be volatilized and eliminated before the slurry is cured, avoiding the occurrence of bubble defects in the pores and obtaining a good sintering morphology.

[0031] Preferably, the mono / diepoxy reactive diluent includes any one or more combinations of propenyl glycidyl ether, ethylene glycol diglycidyl ether, n-butyl glycidyl ether, allyl glycidyl ether, glycidyl methacrylate, vinyl cyclohexene monoepoxide, tertiary carboxylic acid glycidyl ester, and glycerol triglycidyl ether; The inactive diluent includes any one or more combinations of ester solvents, ketone solvents and multifunctional ether ester solvents.

[0032] Preferably, the acidic antioxidant is any one or more combinations of ascorbic acid, formic acid and oxalic acid.

[0033] Preferably, the organic carrier auxiliary agent further comprises a plasticizer; The plasticizer is any one or more combinations of phthalate, tributyl citrate, and polyols with carbon numbers of 2≤C≤6.

[0034] In a second aspect, the present invention further provides a method for preparing the copper paste suitable for PCB hole filling, comprising the following steps: (S.1) drying the copper nanoparticles under an inert gas protection or vacuum environment; (S.2) adding an organic carrier to the copper nanoparticles and mixing and dispersing the mixture thoroughly; (S.3) Grinding with a three-roll mill and filtering to obtain the copper paste suitable for PCB hole filling.

[0035] Therefore, the present invention has the following beneficial effects: (1) The copper paste prepared by this method has a production cost much lower than that of silver paste in the same application scenario, a simple operation process and a good working environment. It can replace the highly polluting acid copper electroplating process in the production of printed electronics industry and has a very high replacement value.

[0036] (2) The method prepares copper powder particles with ligands on the surface by liquid phase reduction method, and obtains copper paste products suitable for PCB hole filling by adding organic carriers and blending with copper particles. The viscosity range of the obtained copper paste is 10Pa·s to 500Pa·s, the resistivity is ≤17.2mΩ·mm (optimum can reach 1.68mΩ·mm) after sintering at 200℃, and the viscosity change range is ≤10% and the resistivity change range is ≤8% when stored at 0-5℃ for 180 days.

[0037] (3) The slurry prepared by this method is prepared by adjusting the type and proportion of organic carriers, selecting different volatile solvents for compounding and adding, and step-wise heating to 200°C for sintering, maintaining a good sintering morphology, with no porosity or cracking defects in the inner and outer regions; the cured adhesion is strong, reaching 5B, and PCB components can be effectively connected.

[0038] (4) The copper paste prepared by this method has a small copper powder particle size (particle size ≤ 1 μm), which is suitable for filling high-precision through holes and blind holes with an aperture of ≤ 100 μm, and the conduction yield is ≥ 95%. It solves the low-precision problem of traditional printing process products to a certain extent, and is expected to achieve the improvement of HDI product performance and production quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a schematic diagram of the conductivity test.

[0040] Figure 2 This is the cross-sectional morphology after hole filling and sintering in Example 1.

[0041] Figure 3 This is the cross-sectional morphology observed by SEM after hole filling and sintering in Example 1.

[0042] Figure 4 This is the cross-sectional morphology of Example 2 after hole filling and sintering.

[0043] Figure 5 This is the cross-sectional morphology of comparative example 1 after hole filling and sintering.

[0044] Figure 6 This is the SEM cross-sectional morphology of comparative example 5 after hole filling and sintering. DETAILED DESCRIPTION

[0045] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments of the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0046] The preparation method of the nano copper particles used in the embodiment of the present invention is as shown in the patent previously applied by the company, "A low-temperature copper slurry suitable for precision 3D printing, its preparation method and application" (CN115188523A). After synthesizing the single copper nanoparticles, they are dried in a vacuum environment for 6 hours to obtain copper nanoparticles with a particle size of ≤1μm.

[0047] Example 1 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh the following by weight: 100 parts of main resin (Epikote 828), 5 parts of curing agent (ACCELERATOR DY 9577), 20 parts of diluent (propylene glycidyl ether), 10 parts of diluent (n-butyl acetate), 20 parts of plasticizer (ethylene glycol), and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0048] (S.2) Take 800 parts of copper powder and 5 parts of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0049] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0050] Example 2 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh 100 parts of main resin (Epikote 828), 3 parts of curing agent (Anchor1115), 20 parts of diluent (propylene glycidyl ether), 10 parts of diluent (diethylene glycol butyl ether acetate), and 10 parts of plasticizer (ethylene glycol) according to weight parts, and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0051] (S.2) Take 500 parts of copper powder and 1 part of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0052] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0053] Example 3 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh 100 parts of the main resin (YD-128), 6 parts of the curing agent (succinic acid dihydrazide), 15 parts of the diluent (ethylene glycol diglycidyl ether), 15 parts of the diluent (n-butyl acetate), and 20 parts of the plasticizer (tributyl citrate) according to weight proportions, and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0054] (S.2) Take 1000 parts of copper powder and 1 part of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0055] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0056] Example 4 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) Under room temperature conditions, weigh 100 parts of the main resin (YD-128), 5 parts of the curing agent (dicyandiamide), 10 parts of the diluent (propylene glycidyl ether), 5 parts of the diluent (isomethyl acetone), and 30 parts of the plasticizer (tributyl citrate) according to their weight parts, and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0057] (S.2) Take 1000 parts of copper powder and 2 parts of reducing agent (oxalic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0058] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0059] Example 5 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh 100 parts of the main resin (TDE-85), 4 parts of the curing agent (dicyandiamide), 6 parts of the curing agent (Anchor1115), 10 parts of the diluent (ethylene glycol diglycidyl ether), 10 parts of the diluent (diethylene glycol butyl ether acetate), 10 parts of the plasticizer (tributyl citrate), and 10 parts of the plasticizer (ethylene glycol) according to their weight parts, and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0060] (S.2) Take 1000 parts of copper powder, 3 parts of reducing agent (ascorbic acid), and 7 parts of reducing agent (hypophosphorous acid) and add them to the organic carrier. Use a mechanical stirrer under a nitrogen atmosphere to mix at a speed of 800 r / min for 20 minutes, and then mix at a speed of 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0061] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0062] Example 6 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh 100 parts of the main resin (TDE-85), 1 part of the curing agent (dicyandiamide), 12 parts of the diluent (n-butyl acetate), and 18 parts of the plasticizer (tributyl citrate) according to their weight proportions, and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0063] (S.2) Take 1200 parts of copper powder and 5 parts of reducing agent (oxalic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0064] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0065] Example 7 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh the following by weight: 100 parts of main resin (Epikote 828), 10 parts of curing agent (ACCELERATOR DY 9577), 30 parts of diluent (propylene glycidyl ether), and 20 parts of plasticizer (ethylene glycol), and stir mechanically at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0066] (S.2) Take 800 parts of copper powder and 5 parts of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0067] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0068] Example 8 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh the following by weight: 100 parts of main resin (Epikote 828), 5 parts of curing agent (ACCELERATOR DY 9577), 5 parts of diluent (propylene glycidyl ether), 5 parts of diluent (isomethyl acetone), 20 parts of plasticizer (ethylene glycol), and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0069] (S.2) Take 800 parts of copper powder and 5 parts of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0070] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0071] Example 9 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh the following by weight: 100 parts of main resin (Epikote 828), 5 parts of curing agent (ACCELERATOR DY 9577), 5 parts of diluent (propylene glycidyl ether), 5 parts of diluent (isomethyl acetone), 5 parts of plasticizer (ethylene glycol), and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0072] (S.2) Take 800 parts of copper powder and 5 parts of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0073] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0074] Example 10 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) At room temperature, weigh the following by weight: 100 parts of main resin (Epikote 828), 5 parts of curing agent (ACCELERATOR DY 9577), 5 parts of diluent (propylene glycidyl ether), 5 parts of diluent (isomethyl acetone), 30 parts of plasticizer (ethylene glycol), and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0075] (S.2) Take 800 parts of copper powder and 5 parts of reducing agent (ascorbic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0076] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0077] Embodiment 11 A method for preparing a copper paste suitable for PCB hole filling comprises the following steps: (S.1) Under room temperature conditions, weigh 100 parts of the main resin (YD-128), 5 parts of the curing agent (dicyandiamide), 10 parts of the diluent (propylene glycidyl ether), 5 parts of the diluent (isomethyl acetone), and 30 parts of the plasticizer (tributyl citrate) according to their weight parts, and use mechanical stirring at room temperature until they are fully dissolved and dispersed to obtain an organic carrier.

[0078] (S.2) Take 3000 parts of copper powder and 2 parts of reducing agent (oxalic acid) and add them to the organic carrier. Use a mechanical stirrer to mix at 800 r / min for 20 minutes under a nitrogen atmosphere, and then mix at 1500 r / min for 10 minutes to ensure that the particles are fully dispersed.

[0079] (S.3) Grind and disperse using a three-roll mill, and use a 300-500 mesh sieve to scrape and filter in a nitrogen environment to obtain a copper slurry suitable for PCB hole filling.

[0080] The formulas of the copper pastes suitable for PCB via filling in Examples 1 to 10 are summarized in Table 1 below.

[0081] Table 1 Note: The unit of addition amount of each substance in the above table is part.

[0082] Comparative Example 1 The comparison was performed according to the formula of Example 1 in patent CN115188523A.

[0083] Comparative Example 2 The remaining components of Comparative Example 2 are consistent with those of Example 1 of the present invention, except that the main resin (Epikote 828) is eliminated in Comparative Example 2, and the addition ratio of copper powder to the remaining components remains unchanged.

[0084] Comparative Example 3 The remaining components of Comparative Example 3 are consistent with those of Example 1 of the present invention, except that in Comparative Example 3, the latent curing agent (ACCELERATOR DY 9577) in Example 1 is replaced by an equal amount of a polyamine curing agent (650 low molecular weight polyamide).

[0085] Comparative Example 4 The remaining components of Comparative Example 4 are consistent with those of Example 1 of the present invention, except that in Comparative Example 4, the medium-boiling-point diluent (propylene glycidyl ether and n-butyl acetate) in Example 1 is replaced by an equal amount of a high-boiling-point diluent (mixed dibasic acid ester).

[0086] Comparative Example 5 The remaining components of Comparative Example 5 are consistent with those of Example 1 of the present invention, except that the use of the plasticizer (ethylene glycol) is eliminated in Comparative Example 5, and the addition ratio of the copper powder to the remaining components remains unchanged.

[0087] Comparative Example 6 The remaining components of Comparative Example 6 are consistent with those of Example 1 of the present invention, except that the reducing agent (ascorbic acid) is omitted in Comparative Example 6, and the addition ratio of copper powder to the remaining components remains unchanged.

[0088] Comparative Example 7 The other components of Comparative Example 7 are consistent with those of Example 1 of the present invention, except that the addition amount of the curing agent (ACCELERATOR DY 9577) in Comparative Example 7 is 15 parts, and the addition ratio of the copper powder to the other components remains unchanged.

[0089] Comparative Example 8 The remaining components of Comparative Example 7 are consistent with those of Example 1 of the present invention, except that in Comparative Example 8, the amount of diluent (propylene glycidyl ether) added is 5 parts, and the amount of diluent (n-butyl acetate) added is 2.5 parts.

[0090] Comparative Example 9 The remaining components of Comparative Example 8 are consistent with those of Example 1 of the present invention, except that in Comparative Example 9, the amount of diluent (propylene glycidyl ether) added is 30 parts, and the amount of diluent (n-butyl acetate) added is 15 parts.

[0091] Comparative Example 10 The remaining components of Comparative Example 10 are consistent with those of Example 1 of the present invention, except that in Comparative Example 10, the acidic ascorbic acid is replaced by weakly alkaline sodium ascorbate.

[0092] Comparative Example 11 The remaining components of Comparative Example 10 are consistent with those of Example 1 of the present invention, except that in Comparative Example 11, ascorbic acid is replaced by hydrazine hydrate.

[0093] Comparative Example 12 The remaining components of Comparative Example 11 are consistent with those of Example 1 of the present invention, except that in Comparative Example 12, the main resin is replaced with resorcinol glycidyl ether, and the thermal expansion coefficient of the cured product thereof is greater than 100 ppm / K.

[0094]

Performance evaluation

[0095] Attached is the test method: (1) Microscopic observation The internal morphology of the filled holes was characterized using a Phenom scanning electron microscope.

[0096] The specific method is: ① Use 1000 mesh coarse sandpaper to pre-polish the PCB; ② Use 5000 mesh fine sandpaper to continue polishing until the cross section is completely exposed; ③ Prepare samples for observation to obtain image information of the internal morphology of the filled holes and evaluate bubbles, pores and edge adhesion.

[0097] (2) Resistivity test The resistivity of copper slurry was measured using a Ruike Weiye FT-340 four-probe square resistance tester.

[0098] The specific method is as follows: ① The prepared copper paste for filling holes is scraped onto the glass original plate through a coating machine, and sintered at 200°C for 60 minutes under a nitrogen atmosphere to obtain a conductive copper film; ② The thickness of the copper film sample after high-temperature sintering is measured with the help of a step meter; ③ The corresponding parameters are set in the square resistance meter, and the four-probe probe is adjusted to press down vertically above the sample to be tested and touch lightly; ④ After the reading is stable, the resistivity and other data are recorded.

[0099] (3) Viscosity test The viscosity of the copper slurry was measured using a Brookfield DVNextCP cone and plate viscometer.

[0100] The specific method is: ① adjust the torque to zero and adjust the vertebral plate spacing to 0.0005 inches; ② take a volume of 0.5ml of copper slurry and place it in the center of the sample cup, set the speed and test time, where the speed is 0.5rpm; ③ start the test to obtain material viscosity information and record it.

[0101] (4) Adhesion test ① The prepared copper paste was scraped onto the PCB substrate by a coating machine and sintered at 200°C for 10 min under a nitrogen atmosphere to obtain a conductive copper film; ② Using ASTM D3359-2017 as the test standard, a grid knife was used to cut the surface of the test piece at a cutting speed of 20-50 mm / s; ③ The test piece was rotated 90° and the above operation was repeated on the cut to form a grid pattern; ④ The diagonal lines on both sides of the grid pattern were brushed lightly 5 times each; ⑤ A special tape peeling test was performed using 3M 600-1PK test, and the adhesion performance of the material was evaluated.

[0102] (5) Conductivity Yield Evaluation ① Such as Figure 1 As shown, 3D direct writing printing is used to fill the 75μm diameter through hole (as shown in the figure 03) in the PCB board (as shown in the figure 01) with slurry. The hole depth is 200μm, the diameter-to-depth ratio is 0.375, and the number of filled holes is 500. ② Print a 2mm×2mm plane with leads on both sides of each through hole (as shown in the figure 02) to form a through-hole circuit. ③ Place the filled hole board in a nitrogen atmosphere for heat treatment at 80℃ for 20min, then heat it at 200℃ for 40min and cool it naturally. ④ Use the positive and negative poles of a multimeter to measure the resistance at both ends of the through hole after curing. If the resistance value is ≤100Ω, it is judged to be conductive, and the number of conductive holes is recorded as A, and the conversion yield Y=(A×100%) / 500.

[0103] The final performance evaluation is shown in Tables 2 and 3.

[0104] Table 2 Evaluation of comprehensive performance of copper paste in Examples 1 to 10 a:○ indicates that the filling performance meets the product requirements, and × indicates that the filling performance does not meet the product requirements Table 3 Evaluation of the comprehensive performance of copper pastes in comparative examples 1 to 12 a:○ indicates that the filling performance meets the product requirements, and × indicates that the filling performance does not meet the product requirements Results and Discussion From Table 2-3, Figure 2-4 According to the test results, the copper paste prepared by the present invention has good cross-sectional morphology after sintering at 200° C. after filling holes, without obvious pores and cracks, and the conduction yield is greater than 95%.

[0105] Among them, the performance test results of Example 1 and Comparative Examples 1-12 are as follows: (1) In Comparative Example 1, the solid content of the copper slurry is only 60%, the proportion of dispersant is high, and more organic matter volatilizes during the sintering process, causing the slurry to shrink. Microscope observation shows that there are many internal pores and cracks after curing ( Figure 5 ).

[0106] (2) In Comparative Example 2, since the main resin was not added, the slurry could not be fully solidified, and the block was still in a plastic state after sintering, and the dispersant component escaped due to heat to produce pores. At the same time, the adhesion of the slurry decreased, and the test resistance increased.

[0107] (3) In comparative example 3, the latent curing agent is replaced with a polyamine curing agent. The selected 650 low molecular weight polyamide promotes the curing of the resin at room temperature through the addition reaction of the active hydrogen of the primary amine and secondary amine with the epoxy group. Therefore, the prepared slurry has a short use window period and is not suitable for actual production scenario application.

[0108] (4) Comparative Example 4 uses a high boiling point diluent mixed dibasic acid ester to replace the acryl glycidyl ether and n-butyl acetate in Example 1. Since the mixed dibasic acid ester has a higher boiling point and a much lower volatilization rate than n-butyl acetate, the slurry is not fully cured at 200°C and finally presents a semi-cured state.

[0109] (5) Since small molecule ethylene glycol can be inserted between polymer molecular chains, the distance between molecular chains is enlarged, chain entanglement is reduced, and the attraction is weakened, thereby increasing the possibility of interchain movement. When no similar components are added, the wettability of organic solvents between copper nanoparticles decreases, and the dispersion and fluidity of the slurry obtained in comparative example 5 are not as good as those in example 1. SEM photography observed that there were obvious cracks inside and on the edges of the cross section after sintering ( Figure 6 ).

[0110] (6) Comparative Example 6 did not introduce a reducing organic carrier additive, and the storage stability of the slurry decreased. This is because the copper nanoparticles are highly active and are easily oxidized to form copper oxide when exposed to water and oxygen in the air. The addition of a reducing weak acid such as ascorbic acid can inhibit the copper oxidation reaction, thereby extending the storage period of the slurry.

[0111] (7) In Example 7, the amount of curing agent added was increased by 3 times, and the storage stability of the slurry was not significantly affected, but the thermal curing speed was significantly increased, and the contact sites between the particles were reduced. The conductive performance was decreased at the same curing time.

[0112] (8) In comparative example 8, the amount of two diluents added was reduced, and the viscosity of the slurry increased significantly, while the fluidity decreased. When filling the holes of the PCB board, the slurry could not be fully infiltrated. When observing the final cured morphology, a large number of residual pores and cracks were found.

[0113] (9) In Example 9, the amount of two diluents added was increased. The slurry had good fluidity and could fully infiltrate the pores. However, due to the escape of the diluent during the thermosetting process, the volume and mass loss of the slurry increased after thermosetting, resulting in the formation of local pores and cracks.

[0114] (10) In Comparative Example 10, acidic ascorbic acid is replaced with weakly alkaline sodium ascorbate. Although sodium ascorbate has reducing properties, it cannot be fully dissolved in the organic carrier and is still dispersed in the form of particles after addition. The obtained slurry has poor uniformity and there is a problem of blockage of the fine outlet.

[0115] (11) In comparative example 11, ascorbic acid is replaced by hydrazine hydrate. Since hydrazine hydrate is a strong reducing agent, it acts on the surface of copper particles and causes excessive reduction. In addition, high concentration of hydrazine hydrate easily absorbs water, causing secondary oxidation of the material when it is exposed to the water and oxygen environment of the air, and the storage stability of the slurry is reduced.

[0116] (12) In comparative example 12, the main resin is replaced with hydroquinone diglycidyl ether. After curing, the slurry overflows along the hole diameter in the hole-filling cross section and there are tiny pores. Due to the increase in volume, the density of the material decreases, resulting in poor conductivity.

[0117] From a comprehensive comparison, the copper paste prepared by the scheme of the present invention has good performance and meets the application requirements of PCB board hole filling scenarios.

Claims

1. A copper paste suitable for PCB hole filling, characterized in that: It consists of copper nanoparticles with ligands on the surface and an organic carrier; wherein: The particle size of the copper nanoparticles is ≤1 μm; The organic carrier includes a main resin, a latent curing agent, a diluent and an organic carrier auxiliary agent; The organic carrier auxiliary agent includes an acidic antioxidant.

2. The copper paste suitable for PCB hole filling according to claim 1, characterized in that: The content of the organic carrier accounts for 5-25% of the total mass of the copper paste, and the content of the copper nanoparticles accounts for ≥75% of the total mass of the copper paste.

3. The copper paste suitable for PCB hole filling according to claim 1 or 2, characterized in that: The organic vehicle comprises, by weight, 100 parts of a single-component main resin, 1 to 10 parts of a latent curing agent, 10 to 30 parts of a diluent, and 10 to 40 parts of an organic vehicle auxiliary agent.

4. The copper paste suitable for PCB hole filling according to claim 1 or 2, characterized in that: The main resin is a thermosetting resin with a thermal expansion coefficient of ≤100 ppm / K.

5. The copper paste suitable for PCB hole filling according to claim 4, characterized in that: The main resin includes any one or more combinations of bisphenol A epoxy resin, bisphenol F epoxy resin, and alicyclic epoxy resin.

6. The copper paste suitable for PCB hole filling according to claim 1, characterized in that: The latent curing agent includes any one or more combinations of dicyandiamide and its derivatives, organic acid hydrazides, and boron trichloride amine complexes.

7. The copper paste suitable for PCB hole filling according to claim 1 or 2, characterized in that: The diluent is a mono- or di-epoxy reactive diluent or an inactive diluent with a boiling point of 80-120°C.

8. The copper paste suitable for PCB hole filling according to claim 7, characterized in that: The mono / diepoxy reactive diluent includes any one or more combinations of propenyl glycidyl ether, ethylene glycol bisglycidyl ether, n-butyl glycidyl ether, allyl glycidyl ether, glycidyl methacrylate, vinyl cyclohexene monoepoxide, tertiary carboxylic acid glycidyl ester, and glycerol triglycidyl ether; The inactive diluent includes any one or more combinations of ester solvents, ketone solvents, and multifunctional ether ester solvents.

9. The copper paste suitable for PCB hole filling according to claim 1 or 2, characterized in that: The acidic antioxidant is an organic acid with a carbon number of ≤10, preferably any one or more of ascorbic acid, formic acid and oxalic acid.

10. The copper paste suitable for PCB hole filling according to claim 9, characterized in that: The organic carrier auxiliary agent also includes a plasticizer; The plasticizer is any one or more combinations of phthalate, tributyl citrate, and polyols with a carbon number of 2≤C≤6.

11. A method for preparing the copper paste suitable for PCB hole filling according to any one of claims 1 to 10, characterized in that: The following steps are involved: (S.1) drying the copper nanoparticles under an inert gas or vacuum environment; (S.2) adding an organic carrier to the copper nanoparticles and thoroughly mixing and dispersing the mixture; (S.3) Grinding with a three-roll mill and then filtering to obtain the copper paste suitable for PCB hole filling.

Citation Information

Patent Citations

  • Electroplating copper plughole process of circuit board

    CN101873770A

  • Grout silver paste used in PCB and preparation method thereof

    CN102262918B

  • Heat-conducting and electric-conducting copper paste as well as preparation method and application thereof

    CN113025230A

  • Plug hole copper paste, preparation method thereof and printed circuit board

    CN114334221A

  • Low-temperature copper paste suitable for high-precision 3D printing as well as preparation method and application of low-temperature copper paste