Conductive silver paste and preparation method thereof

By using multi-scale multi-interface blending technology of micro-nano mixed silver powder, nano-titanium dioxide powder, lead-free glass powder and multi-phase organic binder phase resin in conductive silver paste, the problem of the use of conductive silver paste in the manufacturing of high-temperature sintering electronic components is solved. Solving the problems of high viscosity, low thixotropy and poor adhesion, it achieves high density, low sheet resistance and high adhesion, adapting to various working conditions and continuous production needs.

CN118737522APending Publication Date: 2024-10-01XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411086642.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing conductive silver pastes have problems such as high viscosity, low thixotropy, and poor adhesion in the manufacturing of high-temperature sintered electronic components. They cannot meet the technical requirements of special working conditions, especially under conditions such as deformation and vibration of piezoelectric ceramics. .

Method used

It adopts multi-scale multi-interface blending technology of micro-nano mixed silver powder, nano-titanium dioxide powder, lead-free glass powder and multi-phase organic binder phase resin, combined with multi-component mixed solvents and specific organic additives, to control the viscosity and adhesion of the slurry. Focus on strength and thixotropy, expand the sintering temperature range, and improve the density and stability of the slurry.

Benefits of technology

It achieves high density, low sheet resistance, high adhesion and high stability of conductive silver paste, meets the index requirements of various working conditions, expands the scope of application, and simplifies the coating process to meet the needs of continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737522A_ABST
    Figure CN118737522A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to conductive silver paste and a preparation method of the conductive silver paste, and relates to the technical field of electronic paste, and the conductive silver paste at least comprises the following raw materials: mixed silver powder, organic binding phase resin, a curing agent, nano titanium dioxide powder, lead-free glass powder, an organic solvent and a plurality of auxiliaries. The performance and quality of the conductive silver paste can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The disclosed embodiments relate to the technical field of electronic pastes, and in particular, to a conductive silver paste and a method for preparing the conductive silver paste. Background Art

[0002] High-temperature sintering conductive silver paste has a wide range of applications and plays an important role in the electronic industry manufacturing fields such as solar cells, capacitors, potentiometers, high-voltage / high-frequency ceramic parts, etc. With the rapid advancement of the electronic industrialization process, the technical requirements for high-temperature silver paste in the field of electronic component manufacturing have been improved, especially under special working conditions. Conductive silver paste is required to have high density, high temperature resistance, low square resistance, high adhesion and high stability, and at the same time meet the needs of high environmental protection and low-cost continuous production.

[0003] In the related art, the main components of conductive silver paste are conductive functional fillers, organic carriers, solvents and additives, but the following problems may exist: high viscosity and low thixotropy, poor adhesion, unable to meet the index requirements of various working conditions, and poor quality. Summary of the invention

[0004] The purpose of the present disclosure is to provide a conductive silver paste and a method for preparing the conductive silver paste, thereby overcoming the problem of poor quality of the conductive silver paste due to the limitations and defects of the related art at least to a certain extent.

[0005] According to one aspect of the present disclosure, a conductive silver paste is provided, which comprises at least the following components: mixed silver powder, organic binder phase resin, curing agent, nano titanium dioxide powder, lead-free glass powder, organic solvent and various additives.

[0006] In an exemplary embodiment of the present disclosure, the conductive silver paste comprises at least the following components in parts by weight: 60-85 parts of mixed silver powder, 0.1-5 parts of organic binder phase resin, 0.1-5 parts of curing agent, 1-5 parts of nano titanium dioxide powder, 1-10 parts of lead-free glass powder, 5-20 parts of organic solvent and 0.1-10 parts of various additives.

[0007] In an exemplary embodiment of the present disclosure, the mixed silver powder includes flaky silver powder and spherical silver powder; the flaky silver powder includes flaky silver powder of a first size and flaky silver powder of a second size, and the weight ratio of the flaky silver powder of the first size is greater than the mass ratio of the flaky silver powder of the second size;

[0008] The particle size of the flaky silver powder is 2.0-10.0 μm, the particle size of the spherical silver powder is 5-300 nm, and the ratio of the flaky silver powder to the spherical silver powder is in the range of 9:1-1:1.

[0009] In an exemplary embodiment of the present disclosure, the components of the organic binder phase resin include ethyl cellulose and at least one of a polymer resin; wherein the polymer resin includes a glycidyl ether type epoxy resin, and the curing agent includes at least one of a dicyandiamide, anhydride, and polyamide curing accelerator.

[0010] In an exemplary embodiment of the present disclosure, the particle size of the nano titanium dioxide powder is 50-500 nm.

[0011] In an exemplary embodiment of the present disclosure, the main components of the lead-free glass powder include at least two of silicon oxide, magnesium oxide and zirconium oxide, and the glass transition temperature of the lead-free glass powder is lower than 450°C.

[0012] In an exemplary embodiment of the present disclosure, the components of the organic solvent include at least one of butyl carbitol, terpineol, N-methyl pyrrolidone, alkylbenzene, butyl carbitol acetate and mixed dibasic esters.

[0013] In an exemplary embodiment of the present disclosure, the components of the organic auxiliary agent include at least one of modified urea, polyacrylate, polysiloxane and silane coupling agent, the content of the modified urea is 0.2-1%, the content of the polyacrylate is 0.1-1.5%, the content of the polysiloxane is 0.1-4% and the content of the silane coupling agent is 0.1-4%.

[0014] According to one aspect of the present disclosure, a method for preparing a conductive silver paste is provided, comprising: taking an organic binder phase resin and an organic solvent by weight, mixing and stirring the organic binder phase resin and the organic solvent in a dispersion kettle until they are transparent, so as to obtain an organic carrier; adding lead-free glass powder, nano titanium dioxide powder and silver powder into the dispersion kettle for constant temperature dispersion, so as to prepare a uniform slurry; adding a curing agent and a variety of additives to adjust the slurry viscosity of the uniform slurry, and grinding the slurry with a grinder to adjust the slurry fineness, so as to prepare a conductive silver paste.

[0015] In an exemplary embodiment of the present disclosure, the viscosity of the conductive silver paste is 30-400 Pa·S, and the resistivity of the conductive silver paste is 1.0×10 -6 -3.0×10 -6 Ω / mm, and the sintering temperature of the conductive silver paste is 450-850°C.

[0016] In an exemplary embodiment of the present disclosure, the spacing of the grinder is adjusted to 2-10 μm, and the rotation speed is 300-500 rpm; the rotation speed of the dispersion kettle is 1000-5000 rpm, the dispersion temperature is 65-95° C., and the stirring time is 30-60 minutes.

[0017] In the technical solution provided in the embodiments of the present disclosure, a conductive silver paste including mixed silver powder, organic adhesive phase resin, curing agent, nano titanium dioxide powder, lead-free glass powder, organic solvent and various additives is provided. The conductive silver paste provided in the embodiments of the present disclosure adopts a multi-scale multi-interface blending technology of micro-nano mixed silver powder, nano titanium dioxide powder, lead-free glass powder and organic adhesive phase resin, which improves the compactness of the conductive silver paste, reduces the square resistance of the conductive silver paste, and improves the adhesion and adhesion; adopts a multi-component mixed solvent to avoid the generation of sintering holes and cracks, and improves the quality and stability of the conductive silver paste; configures specific organic additives, and regulates the thixotropy and printing adaptability of the conductive silver paste under the premise of ensuring high temperature resistance, low square resistance and high stability, thereby being able to meet the index requirements of various working conditions, increase the sintering temperature range of the conductive silver paste, can be used under various working conditions, expand the scope of application, and can reduce the difficulty of coating during actual operation to meet the requirements of continuous production.

[0018] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0020] Figure 1 The flowchart schematically shows a method for preparing a conductive silver paste in an embodiment of the present disclosure.

[0021] Figure 2 A schematic diagram schematically illustrates a specific process for preparing conductive silver paste in an embodiment of the present disclosure.

[0022] Figure 3 The result diagram of the performance test of the conductive silver paste in the embodiment of the present disclosure is schematically shown.

[0023] Figure 4 The front scanning electron microscope image of the conductive silver paste prepared in Example 1 of the embodiments of the present disclosure is schematically shown.

[0024] Figure 5 The front scanning electron microscope image of the conductive silver paste prepared in Example 2 of the disclosed embodiments is schematically shown.

[0025] Figure 6 The front scanning electron microscope image of the conductive silver paste prepared in Example 3 of the embodiments of the present disclosure is schematically shown.

[0026] Figure 7 The front scanning electron microscope image of the conductive silver paste prepared in Example 3 of the embodiments of the present disclosure is schematically shown.

[0027] Figure 8 The cross-sectional scanning electron microscope image of the conductive silver paste after sintering is schematically shown. DETAILED DESCRIPTION

[0028] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0029] The terms "a", "an", "the" and "said" used in this specification are used to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components, etc. in addition to the listed elements / components, etc.; the terms "first" and "second" etc. are used only as labels and are not intended to limit the quantity of their objects.

[0030] In some embodiments, the main components of the conductive silver paste are conductive functional fillers, organic carriers, solvents and additives. Although the commonly used high-temperature sintered silver paste products meet the basic technical indicators and have the characteristics of low square resistance and high temperature resistance, they still have the following problems: high viscosity and low thixotropy, difficulty in coating during actual operation, poor printing adaptability, and adhesion needs to be improved, and cannot meet the index requirements of special service conditions such as deformation and vibration of piezoelectric ceramics.

[0031] In order to solve the technical problems in the related art, a conductive silver paste is provided in the embodiment of the present disclosure, and the conductive silver paste includes at least the following raw materials: at least the following components: mixed silver powder, organic binder phase resin, curing agent, nano titanium dioxide powder, lead-free glass powder, organic solvent and various additives. In some embodiments, the conductive silver paste includes the following components by weight: 60-85 parts of mixed silver powder, 0.1-5 parts of organic binder phase resin, 0.1-5 parts of curing agent, 1-5 parts of nano titanium dioxide powder, 1-10 parts of lead-free glass powder, 5-20 parts of organic solvent and 0.1-10 parts of various additives.

[0032] Next, the conductive silver paste in the embodiment of the present disclosure is described in detail.

[0033] In the disclosed embodiment, the conductive silver paste includes the following raw materials in parts by weight: 60-85 parts of mixed silver powder, 0.1-5 parts of organic binder resin, 0.1-5 parts of curing agent, 1-5 parts of nano titanium dioxide powder, 1-10 parts of lead-free glass powder, 5-20 parts of organic solvent and 0.1-10 parts of various additives.

[0034] Wherein, the conductive filler mixed silver powder is selected from silver powders of multiple dimensions and different particle sizes, and the mixed silver powder can be a multi-dimensional micro-nano mixed silver powder, and the mixed silver powder may include silver powders of different shapes, for example, flaky silver powder and spherical silver powder. The particle size of the flaky silver powder may include multiple, which is determined according to actual needs. In some embodiments, the mixed silver powder includes two flaky silver powders and one spherical silver powder, and the particle sizes of the two flaky silver powders may be different. Wherein, the two flaky silver powders include a first-size flaky silver powder and a second-size flaky silver powder, and the particle size of the first-size flaky silver powder is smaller than the particle size of the second-size flaky silver powder. Exemplarily, the particle size of the first-size flaky silver powder is 2.0-5.0 μm, and the particle size of the second-size flaky silver powder is 3.0-10.0 μm. Wherein, the weight ratio of the first-size flaky silver powder is greater than the weight ratio of the second-size flaky silver powder. Spherical silver powder refers to spherical granular silver powder, the particle size of which may be smaller than that of flaky silver powder, and the particle size of spherical silver powder may be 5-300nm. The ratio of flaky silver powder to spherical silver powder in the mixed silver powder is in the range of 9:1-1:1, that is, the ratio of flaky silver powder to spherical silver powder is 9:1-1:1. It should be noted that the weight ratio of flaky silver powder to spherical silver powder can also be adjusted according to actual needs.

[0035] The components of the organic adhesive phase resin may include at least one of ethyl cellulose and a polymer resin. When the organic adhesive phase resin is a polymer resin, the polymer resin may be a glycidyl ether epoxy resin. In some embodiments, the glycidyl ether epoxy resin may include at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, and polyphenol glycidyl ether epoxy resin.

[0036] The curing agent may include at least one of dicyandiamide, acid anhydride, and polyamide curing accelerators. The curing agent may be selected according to different requirements, and the weight of the polymer resin represented by the glycidyl ether epoxy resin may be different from the weight of the curing agent.

[0037] In some embodiments, the crystal form of the nano titanium dioxide powder is rutile, and the crystal form of the nano titanium dioxide powder can also be anatase or brookite. The particle size of the nano titanium dioxide powder is 50-500nm.

[0038] In some embodiments, the lead-free glass powder may be a low-melting-point lead-free glass powder, the main components of which include two or more of silicon oxide, phosphorus oxide, sodium oxide, boron oxide, and aluminum oxide. The composition of the lead-free glass powder may be determined according to actual needs. For example, the lead-free glass powder may include silicon oxide, phosphorus oxide, sodium oxide, boron oxide, and aluminum oxide. Among them, the content of phosphorus oxide is the highest, the content of sodium oxide is less than that of phosphorus oxide, the content of silicon oxide is less than that of sodium oxide, the content of aluminum oxide is less than that of silicon oxide, and the content of boron oxide is the lowest, but the content of each oxide may be adjusted according to actual needs. The glass transition temperature of the lead-free glass powder refers to the temperature corresponding to the transition from the glass state to the highly elastic state, and the glass transition temperature of the lead-free glass powder is lower than 450°C.

[0039] The components of the organic solvent may be at least one of butyl carbitol, terpineol, N-methyl pyrrolidone, alkylbenzene, butyl carbitol acetate and mixed dibasic esters. For example, the organic solvent may include terpineol, butyl carbitol acetate and mixed dibasic esters, and may also include other components, which are not specifically limited here.

[0040] The various additives may be organic additives, which may include modified urea, polyacrylate, polysiloxane and silane coupling agent, wherein the organic additives may include the following components by weight percentage: modified urea 0.2-1%, polyacrylate 0.1-1.5%, polysiloxane 0.1-4% and silane coupling agent 0.1-4%.

[0041] The conductive silver paste in the disclosed embodiment improves the density and adhesion of the paste through the multi-scale and multi-interface blending technology of micro-nano mixed silver powder, nano titanium dioxide powder, lead-free glass powder and multi-phase organic binder phase resin; adopts the gradient volatilization hierarchy of multi-component mixed solvent to avoid the generation of sintering holes and cracks; formulates specific additives to regulate the thixotropy and printing adaptability of the paste while ensuring the high temperature resistance, low square resistance, high adhesion and high stability of the paste, expands the sintering temperature range of the paste, and at the same time can meet the high environmental protection and low cost continuous production requirements.

[0042] In addition, the present disclosure also provides a method for preparing a conductive silver paste. Figure 1As shown in , the preparation method of the conductive silver paste mainly includes the following steps:

[0043] In step S110, an organic binder phase resin and an organic solvent are taken in parts by weight, and the organic binder phase resin and the organic solvent are mixed and stirred in a dispersion kettle until they are in a transparent state to obtain an organic carrier;

[0044] In step S120, lead-free glass powder, nano titanium dioxide powder and mixed silver powder are added into the dispersion kettle for constant temperature dispersion to prepare a uniform slurry;

[0045] In step S130, a curing agent and a plurality of auxiliary agents are added to adjust the viscosity of the uniform slurry, and the slurry is ground by a grinder to adjust the fineness of the slurry to prepare a conductive silver paste.

[0046] In the disclosed embodiment, the dispersion kettle can be a constant temperature high-speed dispersion kettle, the speed of the constant temperature high-speed dispersion kettle is 1000-5000 rpm, the dispersion temperature is controlled at 65-95°C, and the stirring time is 10-60 minutes. The grinder can be a three-roll grinder, the spacing of the three-roll grinder is adjusted to 2-10μm to meet the slurry fineness requirements, and the speed of the three-roll grinder is controlled at 300-500 rpm. Among them, the speed and the spacing of the three-roll grinder can be adjusted according to the actual slurry fineness requirements.

[0047] Based on this, first, the organic adhesive phase resin and the organic solvent can be added to the constant temperature high-speed dispersion kettle, and the organic adhesive phase resin and the organic solvent are mixed and stirred at a speed of 1000-5000 rpm in the constant temperature high-speed dispersion kettle until they are transparent to obtain an organic carrier. After obtaining the organic carrier, the lead-free glass powder, nano titanium dioxide powder and mixed silver powder can be added to the constant temperature high-speed dispersion kettle, and the mixture can be stirred at a speed of 1000-5000 rpm to configure a uniform slurry; further, the curing agent and the organic auxiliary agent can be added, and the mixture can be stirred at a speed of 1000-5000 rpm for 10-60 minutes, and the mixed slurry can be rolled by a three-roll mill, and the speed of the three-roll mill is 300-500 rpm. The roller spacing of the three-roll mill is adjusted so that the slurry fineness meets the requirements, and a conductive silver paste is prepared. It should be noted that when dispersing in the constant temperature high-speed dispersion kettle, the dispersion temperature is controlled at 65-95°C.

[0048] After grinding by a grinder, the prepared conductive silver paste can also be screen printed to print on a ceramic sheet to obtain a sample, and then the sample is dried and sintered to obtain a sample for performance testing. Among them, a 350 mesh screen can be used in the screen printing process, the ceramic sheet can be an alumina ceramic sheet, and the screen printing area can be 1×1 cm. It should be noted that the mesh number of the screen and the screen printing area can be adjusted according to actual needs. When drying, a constant temperature drying oven can be used for drying, the drying temperature is 130°C, and the drying time is 20 minutes. During sintering, sintering can be carried out by a muffle furnace, and the sintering temperature of the conductive silver paste can be 450-850°C, for example, 650°C. The drying temperature, drying time, and sintering temperature, etc. can all be adjusted according to actual needs.

[0049] After being stirred in a dispersion kettle and ground in a three-roll mill, the viscosity of the conductive silver paste is controlled at 30-400 Pa·S, and the resistivity of the conductive silver paste is 1.0×10 -6- 3.0×10 -6 Ω / mm. By adding curing agent and organic additives to adjust the viscosity of the uniform slurry, the thixotropic properties of the uniform slurry can be adjusted. Adjusting the thixotropic properties refers to the change in consistency or fluidity of the conductive slurry as it is dispersed in the dispersion kettle, as long as it meets the requirements.

[0050] On this basis, Figure 2 The specific flow chart of preparing the conductive paste is schematically shown in Figure 2 As shown in , it mainly includes the following steps:

[0051] In step S210, an organic binder phase resin and an organic solvent are added, and the mixture is dispersed at a constant temperature and high speed in a dispersion kettle to obtain an organic carrier;

[0052] In step S220, the multi-dimensional micro-nano mixed silver powder is added to the organic carrier in batches in small amounts and multiple times, and the nano titanium dioxide powder and the low melting point lead-free glass powder are added to the dispersion kettle for constant temperature and high-speed dispersion to prepare a uniform slurry;

[0053] In step S230, a curing agent and an organic auxiliary agent are added, dispersed at a high speed and ground by three rollers to obtain a high-temperature sintered conductive silver paste.

[0054] During the preparation of the conductive paste, any component of the conductive paste can be adjusted, for example, the component can be selected from multiple raw materials included in each component to adjust the type of component or keep the component unchanged and adjust the weight of the component, which is not specifically limited here.

[0055] The preparation method of the conductive silver paste provided by the present disclosure adopts a multi-scale multi-interface blending technology of micro-nano mixed silver powder, titanium dioxide nanopowder, lead-free glass powder and multi-phase organic bonding phase to improve the density and adhesion of the paste; adopts the gradient volatilization hierarchy of the multi-component mixed solvent to avoid the generation of sintering holes and cracks; formulates specific organic additives, and regulates its thixotropy and printing adaptability under the premise of ensuring the high temperature resistance, low square resistance, high adhesion and high stability of the paste, expands the sintering temperature range of the paste, and meets its high environmental protection and low-cost continuous production requirements. The coating operation is simplified, the printing adaptability is improved, the adhesion is improved, and the index requirements of special working conditions such as deformation and vibration of piezoelectric ceramics can be met.

[0056] Next, the conductive silver paste and the preparation method of the conductive silver paste are specifically described in conjunction with the embodiments.

[0057] Example 1

[0058] In the embodiment of the present disclosure, the raw materials include the following components by weight: 65 parts of mixed silver powder, 5 parts of glycidyl ether epoxy resin E51, 1 part of dicyandiamide, 2 parts of 100nm titanium dioxide powder, 3 parts of lead-free glass powder, 17 parts of organic solvent, and 7 parts of organic auxiliary additives. Among them, the mixed silver powder includes first-size flaky silver powder and second-size flaky silver powder. Based on this, the mixed silver powder includes 20 parts of 7.5μm flaky silver powder, 35 parts of 2.5μm flaky silver powder and 10 parts of 300nm spherical silver powder; the main components of the lead-free glass powder include 14% silicon dioxide, 60% phosphorus pentoxide, 3% boron oxide, 16% sodium oxide and 7% aluminum oxide. The particle size of the low-melting point lead-free glass powder is 4μm, and the glass transition temperature is 450℃. The organic solvent includes 5 parts of pine alcohol, 2 parts of butyl carbitol acetate and 10 parts of mixed dibasic esters; the organic auxiliary additives include 1 part of modified urea, 1.5 parts of polyacrylate, 0.5 parts of polysiloxane and 4 parts of silane coupling agent. Among them, the organic bonding phase resin is 5 parts of glycidyl ether type epoxy resin E51, and the curing agent is 1 part of dicyandiamide.

[0059] The preparation process of the conductive silver paste in the embodiment of the present disclosure includes the following steps:

[0060] Step 1: Take 5 parts of epoxy resin E51 and 17 parts of organic solvent by weight, mix and stir in a high-speed dispersing kettle at 75° C. at 1000 rpm until transparent, to obtain an organic carrier;

[0061] Step 2, weigh 3 parts of lead-free glass powder, 2 parts of 100nm titanium dioxide powder and 65 parts of mixed silver powder, add 3 parts of lead-free glass powder, 2 parts of 100nm titanium dioxide powder and 65 parts of mixed silver powder into a constant temperature high-speed dispersing kettle, and continue stirring to prepare a uniform slurry;

[0062] Step 3: Continue to add 7 parts of organic additives and 1 part of dicyandiamide, and after high-speed dispersion and stirring for 10 minutes, roll the mixed slurry through a three-roll mill, and adjust the roller spacing to make the slurry fineness reach 5μm, so as to prepare a conductive silver paste with high adhesion and low square resistance. The slurry fineness can be set according to actual needs and adjusted by adjusting the three-roll mill.

[0063] Step 4: Print the prepared conductive silver paste on the alumina ceramic sheet through a 350 mesh screen. The screen printing area can be 1×1 cm. Place the printed sample in a 130°C constant temperature drying oven and dry it for 20 minutes. Then put it in a muffle furnace and heat sinter it at 650°C, then take it out for performance testing.

[0064] Example 2

[0065] In the disclosed embodiment, the components of the conductive silver paste include the following ingredients by weight: 65 parts of mixed silver powder, 3 parts of epoxy resin E51, 2 parts of bisphenol F epoxy resin HS-170, 1 part of polyamide 650, 2 parts of 100nm titanium dioxide powder, 3 parts of lead-free glass powder, 17 parts of mixed solvent, and 7 parts of organic additives. Among them, the mixed silver powder includes a first-size flaky silver powder and a second-size flaky silver powder. Based on this, the mixed silver powder includes 20 parts of 7.5μm flaky silver powder, 35 parts of 2.5μm flaky silver powder, and 10 parts of 300nm spherical silver powder. The main components of the lead-free glass powder include 14% silicon dioxide, 60% phosphorus pentoxide, 3% boron oxide, 16% sodium oxide, and 7% aluminum oxide. The particle size of the lead-free glass powder is about 4μm, and the glass transition temperature is 450°C. The organic solvent includes 5 parts of pineol, 2 parts of butyl carbitol acetate and 10 parts of mixed dibasic esters; the organic auxiliary additives include 1 part of modified urea, 1.5 parts of polyacrylate, 0.5 parts of polysiloxane and 4 parts of silane coupling agent. Among them, the organic bonding phase resin is 3 parts of epoxy resin E51, 2 parts of bisphenol F epoxy resin HS-170, and the curing agent is 1 part of polyamide 650, that is, the organic bonding phase resin adopts a mixed epoxy resin.

[0066] The preparation process of the conductive silver paste in the embodiment of the present disclosure includes the following steps:

[0067] Step 1: 3 parts of epoxy resin E51, 2 parts of bisphenol F epoxy resin HS-170 and 17 parts of organic solvent are mixed and stirred in a high-speed dispersion kettle at 75° C. at 1000 rpm until transparent to obtain an organic carrier;

[0068] Step 2, weigh 3 parts of lead-free glass powder, 2 parts of 100nm titanium dioxide powder and 65 parts of mixed silver powder into a constant temperature high-speed dispersion kettle, and continue stirring to prepare a uniform slurry;

[0069] Step 3, continue to add 7 parts of organic additives and 1 part of polyamide 650, and after high-speed dispersion stirring for 10 minutes, the mixed slurry is rolled by a three-roll mill, and the roller spacing is adjusted to make the slurry fineness reach 5 μm, to prepare the final conductive silver paste with high adhesion and low square resistance;

[0070] Step 4: Print the prepared conductive silver paste on the alumina ceramic sheet through a 350 mesh screen. The screen printing area during the screen printing process is 1×1 cm. Place the printed sample in a 130°C constant temperature drying oven and dry it for 20 minutes. Then place it in a muffle furnace and heat sinter it at 650°C, then take it out for performance testing.

[0071] Example 3

[0072] In the disclosed embodiment, the raw materials include the following components by weight: 65 parts of mixed silver powder, 5 parts of epoxy resin E51, 1 part of dicyandiamide, 2 parts of 100nm titanium dioxide powder, 3 parts of lead-free glass powder, 17 parts of mixed solvent, and 7 parts of organic additives. Among them, the mixed silver powder includes first-size flaky silver powder and second-size flaky silver powder. Based on this, the mixed silver powder includes 20 parts of 7.5μm flaky silver powder, 35 parts of 2.5μm flaky silver powder and 10 parts of 300nm spherical silver powder. The main components of the lead-free glass powder include 14% silicon dioxide, 60% phosphorus pentoxide, 3% boron oxide, 16% sodium oxide and 7% aluminum oxide. The particle size of the low-melting point lead-free glass powder is 4μm, and the glass transition temperature is 450°C. The organic solvent includes 5 parts of pine alcohol, 2 parts of butyl carbitol acetate and 10 parts of mixed dibasic esters; the organic auxiliary additives include 1 part of organic bentonite, 1.5 parts of polyacrylate, 0.5 parts of polysiloxane and 4 parts of silane coupling agent. Among them, the organic bonding phase resin is 5 parts of glycidyl ether type epoxy resin E51, the curing agent is 1 part of dicyandiamide, and the organic auxiliary is 1 part of organic bentonite.

[0073] The preparation process of the conductive silver paste in the embodiment of the present disclosure includes the following steps:

[0074] Step 1: 5 parts of epoxy resin E51 and 17 parts of organic solvent were mixed and stirred in a high-speed dispersion kettle at 75° C. at 1000 rpm until transparent to obtain an organic carrier;

[0075] Step 2, weigh 3 parts of lead-free glass powder, 2 parts of 100nm titanium dioxide powder and 65 parts of mixed silver powder into a constant temperature high-speed dispersion kettle, and continue stirring to prepare a uniform slurry;

[0076] Step 3, continue to add 7 parts of organic additives and 1 part of dicyandiamide, and after high-speed dispersion stirring for 10 minutes, the mixed slurry is rolled by a three-roll mill, and the roller spacing is adjusted to make the slurry fineness reach 5 μm, to prepare the final conductive silver paste with high adhesion and low square resistance;

[0077] Step 4: Print the prepared conductive silver paste on the alumina ceramic sheet through a 350-mesh screen. The screen printing area during the screen printing process is 1×1 cm. Place the printed sample in a 130°C constant temperature drying oven and dry it for 20 minutes. Then place it in a muffle furnace and sinter it at 650°C. Then take it out for performance testing.

[0078] Example 4

[0079] In the disclosed embodiment, the raw materials include the following components by weight: 75 parts of mixed silver powder, 5 parts of epoxy resin E51, 1 part of dicyandiamide, 2 parts of 100nm titanium dioxide powder, 3 parts of lead-free glass powder, 17 parts of mixed solvent, and 7 parts of organic additives. Among them, the mixed silver powder includes first-size flaky silver powder and second-size flaky silver powder. Based on this, the mixed silver powder includes 25 parts of 7.5μm flaky silver powder, 35 parts of 2.5μm flaky silver powder and 15 parts of 300nm spherical silver powder. The main components of the lead-free glass powder include 14% silicon dioxide, 60% phosphorus pentoxide, 3% boron oxide, 16% sodium oxide and 7% aluminum oxide. The particle size of the lead-free glass powder is about 4μm, and the glass transition temperature is 450°C. The organic solvent includes 5 parts of pine alcohol, 2 parts of butyl carbitol acetate and 10 parts of mixed dibasic esters; the organic auxiliary additives include 1 part of modified urea, 1.5 parts of polyacrylate, 0.5 parts of polysiloxane and 4 parts of silane coupling agent. Among them, the proportion of small-size spherical silver powder is increased.

[0080] The preparation process of the conductive silver paste in the embodiment of the present disclosure includes the following steps:

[0081] Step 1: 5 parts of epoxy resin E51 and 17 parts of organic solvent were mixed and stirred in a high-speed dispersion kettle at 75° C. at 1000 rpm until transparent to obtain an organic carrier;

[0082] Step 2, weigh 3 parts of low melting point lead-free glass powder, 2 parts of 100nm titanium dioxide powder and 75 parts of mixed silver powder into a constant temperature high-speed dispersion kettle, and continue stirring to prepare a uniform slurry;

[0083] Step 3: Continue to add 7 parts of organic auxiliary additives and 1 part of dicyandiamide, and after high-speed dispersion stirring for 10 minutes, roll the mixed slurry through a three-roll grinder, and adjust the roller spacing so that the slurry fineness reaches 5 μm to prepare the final conductive silver paste with high adhesion and low square resistance.

[0084] Step 4: Print the prepared silver paste on the alumina ceramic sheet through a 350-mesh screen. The screen printing area during the screen printing process is 1×1 cm. Place the printed sample in a 130°C constant temperature drying oven and dry it for 20 minutes. Then place it in a muffle furnace and sinter it at 650°C. Then take it out for performance testing.

[0085] Next, the performance test of the conductive silver paste prepared according to the preparation method in Example 1 to Example 4 may include fineness test, viscosity test, square resistance test and adhesion test. Figure 3 The test results shown in show that the conductive silver paste prepared in Example 3 has the best printing adaptability, and the conductive silver paste prepared in Example 4 has the least holes, the highest sintering density, the largest viscosity, and the smallest square resistance. The adhesion of the high-temperature sintering conductive silver paste prepared in the embodiments of the present disclosure is 5B, so the prepared conductive silver pastes all have high adhesion and low square resistance characteristics, meeting the technical assessment index values.

[0086] refer to Figure 4-Figure 7 From the front scanning electron microscope image of the conductive silver paste sintering shown in , it can be seen that compared with Example 1, the curing time of the conductive silver paste prepared by the mixed epoxy resin in Example 2 is reduced, but the sintering density of the paste deteriorates, the number of holes increases, and the adhesion is 5B, so the adhesion does not change significantly, and it has a relatively high adhesion. The conductive silver paste prepared by adding organic bentonite in Example 3 has excellent thixotropy, good printing adaptability, and improved sintering density of the paste. The conductive silver paste prepared by increasing the proportion of small-particle spherical silver powder in Example 4 has a lower square resistance and higher sintering density. In summary, the conductive silver paste prepared by the embodiments of the present disclosure exhibits low square resistance, high adhesion and good sintering density after high-temperature sintering.

[0087] refer to Figure 8 From the cross-sectional scanning electron microscope image of the conductive paste after sintering shown in FIG, it can be seen that the conductive silver paste layer prepared by the preparation method in the embodiment of the present disclosure is as follows: Figure 8 The silver paste sintered layer shown in the figure has no pores on the interface with the alumina ceramic substrate and the adhesion interface is relatively flat. Therefore, it can be considered that the conductive silver paste has good adhesion and excellent thixotropy.

[0088] The technical solution in the disclosed embodiments provides a high-temperature conductive silver paste that meets the requirements of low square resistance, high hardness, high temperature resistance and high adhesion. The conductive silver paste has good sintering density, and also has the characteristics of high environmental protection, excellent thixotropy and wide temperature sintering range. It simplifies the preparation process of the conductive silver paste, improves the preparation efficiency, and can realize large-scale production.

[0089] In this exemplary embodiment, a target device is also provided. The target device can be any type of device using the conductive silver paste, such as a mobile phone, a tablet computer, a laptop computer, a smart bracelet, a smart watch, a smart helmet, smart glasses, a vehicle, a robot, and any type of electronic device and any type of industrial equipment, etc. As long as the conductive silver paste is used in the target device, this exemplary embodiment does not specifically limit this.

[0090] It should be noted that the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0091] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.

[0092] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A conductive silver paste, characterized in that: The conductive silver paste at least comprises the following components: mixed silver powder, organic bonding phase resin, curing agent, nano titanium dioxide powder, lead-free glass powder, organic solvent and various additives.

2. The conductive silver paste according to claim 1, characterized in that: The conductive silver paste comprises at least the following components in parts by weight: 60-85 parts of mixed silver powder, 0.1-5 parts of organic binder phase resin, 0.1-5 parts of curing agent, 1-5 parts of nano titanium dioxide powder, 1-10 parts of lead-free glass powder, 5-20 parts of organic solvent and 0.1-10 parts of various additives.

3. The conductive silver paste according to claim 1, characterized in that: The mixed silver powder includes flaky silver powder and spherical silver powder; the flaky silver powder includes flaky silver powder of a first size and flaky silver powder of a second size, and the weight ratio of the flaky silver powder of the first size is greater than the mass ratio of the flaky silver powder of the second size; The particle size of the flaky silver powder is 2.0-10.0 μm, the particle size of the spherical silver powder is 5-300 nm, and the ratio of the flaky silver powder to the spherical silver powder is in the range of 9:1-1:

1.

4. The conductive silver paste according to claim 1, characterized in that: The components of the organic bonding phase resin include at least one of ethyl cellulose and a polymer resin; wherein the polymer resin includes a glycidyl ether epoxy resin, and the curing agent includes at least one of a dicyandiamide, anhydride, and polyamide curing accelerator.

5. The conductive silver paste according to claim 2, characterized in that: The particle size of the nano titanium dioxide powder is 50-500nm.

6. The conductive silver paste according to claim 1, characterized in that: The main components of the lead-free glass powder include at least two of silicon oxide, phosphorus oxide, sodium oxide, boron oxide and aluminum oxide, and the glass transition temperature of the lead-free glass powder is lower than 450°C.

7. The conductive silver paste according to claim 1, characterized in that: The components of the organic auxiliary agent include at least one of modified urea, polyacrylate, polysiloxane and silane coupling agent, wherein the content of the modified urea is 0.2-1%, the content of the polyacrylate is 0.1-1.5%, the content of the polysiloxane is 0.1-4% and the content of the silane coupling agent is 0.1-4%.

8. A method for preparing a conductive silver paste, for preparing the conductive silver paste as claimed in any one of claims 1 to 7, characterized in that: include: Taking an organic binder phase resin and an organic solvent in parts by weight, mixing and stirring the organic binder phase resin and the organic solvent in a dispersion kettle until they are transparent, so as to obtain an organic carrier; Adding lead-free glass powder, nano titanium dioxide powder and mixed silver powder into the dispersion kettle for constant temperature dispersion to prepare a uniform slurry; A curing agent and a variety of additives are added to adjust the viscosity of the uniform slurry, and the slurry is ground by a grinder to adjust the fineness of the slurry to prepare a conductive silver paste.

9. The method for preparing a conductive silver paste according to claim 8, characterized in that: The viscosity of the conductive silver paste is 30-400 Pa·S, and the resistivity of the conductive silver paste is 1.0×10 -6 -3.0×10 -6 Ω / mm, and the sintering temperature of the conductive silver paste is 450-850°C.

10. The method for preparing a conductive silver paste according to claim 8, characterized in that: The spacing of the grinding machine is adjusted to 2-10 μm, and the rotation speed is 300-500 rpm; the rotation speed of the dispersion kettle is 1000-5000 rpm, the dispersion temperature is 65-95° C., and the stirring time is 30-60 minutes.

Citation Information

Cited By

  • Silver paste, preparation method thereof and photovoltaic cell

    CN119626628A

  • Conductive silver paste for low-temperature co-fired ceramic and preparation method of conductive silver paste

    CN119694628A

  • Silver paste for photovoltaic cell and preparation method of silver paste for photovoltaic cell

    CN121790055A

  • Silver paste for photovoltaic cell and method for preparing silver paste for photovoltaic cell

    CN121790055B