Inductor
By designing a wound rectangular wire and a magnetic powder resin body in a small inductor, and adjusting the structural parameters, the Isat/Rdc ratio is improved, which solves the shortcomings of existing inductors in optimizing DC characteristics and achieves better inductors. device performance.
Patent Information
- Application Number
- CN202410196891.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-01
AI Technical Summary
Existing small inductors have deficiencies in parameter setting in optimizing DC superimposed rated current and DC resistance, making it difficult to meet specific characteristic requirements.
An inductor is designed. Its coil is composed of wound rectangular wires. The green body contains magnetic powder and resin. By adjusting the structural parameters of the green body such as side gap and peripheral area, the K value is calculated to be above 70 and below 110. To improve the ratio of Isat/Rdc.
The characteristics of the inductor are optimized, the ratio of Isat/Rdc is increased, and good inductor characteristics are provided, which is suitable for circuits and electronic equipment flowing with large currents.
Smart Images

Figure CN118737655A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to inductors. Background Art
[0002] Patent Document 1 discloses a surface mount inductor including a molded body having a coil formed by winding a conducting wire and a base body using a sealing material containing a resin and a magnetic material.
[0003] Patent Document 1: Japanese Patent Application Publication No. 2010-245473
[0004] In this type of inductor, the area inside the inner periphery of the coil in the green body and the area outside the outer periphery of the coil in the green body are conventionally designed to satisfy the required DC superposition rated current and DC resistance. However, in particular, in an inductor having a small green body, even if these parameters are optimized as conventionally, it is difficult to satisfy the required characteristics, and there is room for improvement in parameter setting. Summary of the invention
[0005] One embodiment of the present invention is an inductor, comprising: a coil having a winding portion and a pair of lead portions, wherein the winding portion is formed by winding a rectangular wire, and the pair of lead portions are led out from the winding portion; a blank containing magnetic powder and resin, and having the coil built therein; and an external terminal formed on a surface of the blank and connected to the lead portions, wherein the blank has: a main surface intersecting with a winding axis of the coil and having a rectangular shape having sides along a first direction and a second direction; a pair of first surfaces adjacent to the main surface and along the first direction; a pair of second surfaces adjacent to the main surface and along the second direction; first side gap portions formed on the first side and the second side, respectively. between the outer periphery of the winding portion and the pair of first surfaces; and the second side gap portions are respectively formed between the outer periphery and the pair of second surfaces, when the area of the main surface is set to S1, the total size of the second direction of each of the first side gap portions is set to WSG, the total size of the first direction of each of the second side gap portions is set to LSG, the area of the inner side of the inner periphery of the winding portion when viewed from a direction perpendicular to the main surface is set to S3, the area between the outer periphery and the outer edge of the blank is set to S4, and SG is set to the value obtained by the following formula (A), K obtained by the following formula (B) is greater than 70 and less than 110,
[0006] SG=WSG×LSG (A)
[0007] K = (S1 / SG) x (S4 / S3) (B).
[0008] According to the present invention, an inductor having good characteristics can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 This is a perspective view of the inductor according to the first embodiment of the present invention as viewed from the upper surface side.
[0010] Figure 2 This is a perspective view of the inductor according to the first embodiment as viewed from the bottom surface side.
[0011] Figure 3 This is a perspective view showing the internal structure of the inductor according to the first embodiment.
[0012] Figure 4 This is a schematic diagram of the manufacturing process of the inductor according to the first embodiment.
[0013] Figure 5 This is a schematic diagram showing the green body of the first embodiment as viewed from a direction perpendicular to the upper surface.
[0014] Figure 6 It is a graph showing various parameters and calculated value K in the simulation of the embodiment.
[0015] Figure 7 This is a graph showing the relationship between the value K and Isat / Rdc in the simulation of the embodiment.
[0016] Figure 8 This is a graph showing the relationship between the value K and Isat / Rdc in the simulation of the embodiment.
[0017] Fig. 9 This is a perspective view of the blank according to the second embodiment.
[0018] Fig.10 This is a schematic diagram showing the body of the second embodiment as viewed from a perspective in a direction perpendicular to the upper surface.
[0019] Fig.11 This is a perspective view of a blank according to the third embodiment.
[0020] Fig.12 It is a schematic diagram showing the green body viewed from the bottom surface side.
[0021] Description of Reference Numerals
[0022] 1…inductor, 2…basis, 2a…outer edge, 4…external electrode (external terminal), 10…bottom surface (main surface), 12…upper surface (main surface), 14…end surface (second surface), 16…side surface (first surface), 20…coil conductor (coil), 22…winding portion, 22c…outer periphery, 22d…inner periphery, 23…lead portion, 30…core, 30a…first side gap portion, 30b…first side gap portion, 30c…second side gap portion, 30d…second side gap portion, 102…basis, 123…lead portion, 123a…cross section, 202…basis, 223…lead portion, 223a…surface, Q…winding axis. DETAILED DESCRIPTION
[0023] [Implementation Method 1]
[0024] Hereinafter, a method for manufacturing the inductor 1 and the inductor 1 according to the first embodiment will be described.
[0025] (Overall structure of inductor)
[0026] Figure 1 is a perspective view of the inductor 1 according to the present embodiment as viewed from the upper surface 12 side. Figure 2 It is a perspective view of the inductor 1 as viewed from the bottom surface 10 side.
[0027] The inductor 1 of the present embodiment is configured as a surface-mount electronic component and includes a substantially rectangular parallelepiped green body 2 which is one form of a substantially hexahedral shape and a pair of external electrodes (external terminals) 4 provided on the surface of the green body 2 .
[0028] Hereinafter, in the blank 2, the first principal surface facing the mounting substrate (not shown) during mounting is defined as the bottom surface (principal surface) 10, the second principal surface opposite to the bottom surface 10 is referred to as the upper surface (principal surface) 12, the pair of outer surfaces orthogonal to the bottom surface 10 is referred to as the end surface (second surface) 14, and the pair of outer surfaces orthogonal to the bottom surface 10 and the pair of end surfaces 14 is referred to as the side surface (first surface) 16. The pair of end surfaces 14 are arranged to face each other. In addition, the pair of side surfaces 16 are arranged to face each other. The bottom surface 10, the upper surface 12, the end surface 14, and the side surface 16 are respectively substantially rectangular in shape.
[0029] like Figure 1As shown, the distance from the bottom surface 10 to the upper surface 12 is defined as the thickness T of the blank 2, the distance between the pair of side surfaces 16 is defined as the width W of the blank 2, and the distance between the pair of end surfaces 14 is defined as the length L of the blank 2. In addition, the direction of the thickness T is defined as the thickness direction DT, the direction of the width W is defined as the width direction (second direction) DW, and the direction of the length distance is defined as the length direction (first direction) DL. That is, the bottom surface 10 and the upper surface 12 are along the width direction DW and the length direction DL, the end surface 14 is along the width direction DW and the thickness direction DT, and the side surface 16 is along the length direction DL and the thickness direction DT. In addition, the end surface 14 is adjacent to the bottom surface 10, the upper surface 12, and the pair of side surfaces 16. The side surface 16 is adjacent to the bottom surface 10, the upper surface 12, and the pair of end surfaces 14.
[0030] The nominal dimensions of the finished inductor 1 are, for example, a length L of 1.4 mm, a width W of 1.2 mm, and a thickness T of 0.65 mm.
[0031] Hereinafter, the plane along the DL direction and the DT direction is referred to as the LT plane, the plane along the DT direction and the DW direction is referred to as the TW plane, and the plane along the DL direction and the DW direction is referred to as the LW plane. In addition, the cross sections of the inductor 1 along the LT plane, the TW plane, and the LW plane are referred to as the LT cross section, the TW cross section, and the LW cross section, respectively.
[0032] Figure 3 It is a perspective view showing the internal structure of the inductor 1 .
[0033] The base body 2 includes a coil conductor (coil) 20 and a substantially hexahedral core 30 in which the coil conductor 20 is embedded, and is configured as a molded inductor in which the coil conductor 20 is sealed in the core 30 .
[0034] The core body 30 is a molded body that is formed into a substantially hexahedral shape by pressurizing and heating a mixed powder obtained by mixing magnetic particles (magnetic powder) and a resin in a state where the coil conductor 20 is enclosed.
[0035] In addition, the magnetic particles of the present embodiment are formed of a soft magnetic body, and include two types of particles, namely, first magnetic particles of large particles with a relatively large average particle size and second magnetic particles of small particles with a relatively small average particle size. Thus, during compression molding, the second magnetic particles of small particles enter between the first magnetic particles of large particles together with the resin, thereby increasing the filling rate of the magnetic particles in the core 30 and also improving the magnetic permeability.
[0036] In this embodiment, the average particle size of the metal particles of the first magnetic particles is greater than 20 μm and less than 28 μm, and the average particle size of the metal particles of the second magnetic particles is greater than 1 μm and less than 6 μm. In addition, the average particle size of the first magnetic particles is preferably greater than 21.4 μm and less than 27.4 μm, and the average particle size of the second magnetic particles is preferably greater than 1.5 μm and less than 1.8 μm. In addition, the magnetic particles may also include particles having an average particle size different from that of the first magnetic particles and the second magnetic particles, and particles of three or more particle sizes.
[0037] The first magnetic particle and the second magnetic particle are particles having a metal particle, an oxide film covering the surface of the metal particle, and an insulating film covering the surface of the oxide film. The metal particle is covered with the oxide film and the insulating film, so that the insulation resistance and the withstand voltage can be improved.
[0038] In the first magnetic particle of the present embodiment, the metal particle uses Fe-Si-B amorphous alloy powder. The oxide film of the first magnetic particle is composed of two layers of SiO layer and Fe2SiO4, and the thickness of the oxide film as a whole is greater than 20nm and less than 155nm. In addition, the insulating film of the first magnetic particle is formed of phosphate glass with a thickness of greater than 10nm and less than 50nm.
[0039] In addition, in the second magnetic particles of the present embodiment, carbonyl iron powder is used as the metal particle. The oxide film of the second magnetic particle is iron oxide formed by surface oxidation of the carbonyl iron powder as the metal particle. In addition, the insulating film of the second magnetic particle is a sol-gel reaction product with silicon dioxide as a component. As a result, the slippage of the surface of the second magnetic particle is improved, and the second magnetic particle can be easily inserted between the first magnetic particles during the blank forming / curing process of the blank 2 described later. As a result, the density of the magnetic material in the core 30 can be further increased, and the relative magnetic permeability of the core 30 can be further increased.
[0040] Furthermore, in the first magnetic particles, the metal particles may be Fe—Si—Cr alloy powder, Fe—Ni—Al alloy powder, Fe—Cr—Al alloy powder, Fe—Si—Al alloy powder, Fe—Ni alloy powder, or Fe—Ni—Mo alloy powder.
[0041] In the first magnetic particle, the insulating film may be made of phosphoric acid, zinc phosphate, manganese phosphate, glass, or resin.
[0042] The material of the resin contained in the mixed powder of the present embodiment includes bisphenol A type epoxy resin and rubber modified epoxy resin. Thus, the inductor 1 having both improved strength and toughness of the green body 2 can be manufactured.
[0043] In this embodiment, the magnetic powder contained in the mixed powder is based on the total weight of the magnetic particles contained in the mixed powder, and the first magnetic particles are 70wt% or more and 85wt% or less, and the second magnetic particles are 15wt% or more and 30wt% or less. In addition, the resin contained in the mixed powder is based on the total weight of the magnetic powder and the resin, and is 2.0wt% or more and 3.5wt% or less. In addition, the first magnetic particles are preferably 70wt% or more and 80wt% or less, and the second magnetic particles are preferably 20wt% or more and 30wt% or less. In addition, the resin is preferably 2.7wt% or more and 30wt% or less.
[0044] like Figure 3 As shown, the coil conductor 20 includes a winding portion 22 and a pair of lead portions 23, wherein the winding portion 22 is formed by a conductive wire wound around the winding axis Q in a spiral shape at two levels, such that both ends are located at the outer periphery and are connected to each other at the inner periphery, and the pair of lead portions 23 are led out from the winding portion 22. A pair of external electrode connection areas 24 are formed in each lead portion 23, and the pair of external electrode connection areas 24 are conductive wire portions for connecting to external electrodes described later. The winding portion 22 includes two winding areas 22a and 22b that overlap along the winding axis Q. The winding areas 22a and 22b are connected to each other's conductive wires at a portion of their inner peripheries.
[0045] The coil conductor 20 is embedded in the base body 2 such that the winding axis Q is along the thickness direction DT of the base body 2 . That is, the winding axis Q is perpendicular to the bottom surface 10 and the upper surface 12 , and extends in the direction along the end surface 14 and the side surface 16 .
[0046] The wire constituting the coil conductor 20 is composed of a conductor and a covering layer formed on the surface of the conductor. The wire is a rectangular flat wire with a rectangular cross section, and the conductor is a strip conductor with a rectangular cross section made of copper. The thickness of the conductor is greater than 52 μm and less than 118 μm, and the width is greater than 110 μm and less than 180 μm. The covering layer is composed of an insulating layer formed on the surface of the strip conductor and a welding layer formed on the surface of the insulating layer for bonding the strip conductors overlapped in the winding portion 22. The insulating layer is composed of, for example, polyimide amide resin and has a thickness of 3 μm. In addition, the welding layer is composed of, for example, polyamide resin and has a thickness of greater than 1 μm and less than 25 μm.
[0047] The lead portion 23 is led out from the wound portion 22 , and is electrically connected to the external electrode 4 via an external electrode connection region 24 that is exposed by being led out to each of the pair of end faces 14 .
[0048] The pair of external electrodes 4 are so-called L-shaped electrodes consisting of L-shaped members extending from each of the end faces 14 of the base body 2 to the bottom face 10. The external electrodes 4 are connected to the external electrode connection region 24 of the coil conductor 20 at the end faces 14, and a portion 4A ( Figure 2 ) is electrically connected to the wiring of the circuit substrate through appropriate mounting means such as solder.
[0049] In addition, a body protective layer (not shown) is formed on the surface of the body 2 except for the range of the external electrode 4. The body protective layer is, for example, a resin obtained by adding a phenoxy resin to a novolac resin, and contains nano-silica as a filler. The body protective layer is formed on the surface of the body 2 with a thickness of 10 μm or more and 30 μm or less. In addition, the thickness of the body protective layer is preferably 10 μm or more and 20 μm or less, and more preferably 15 μm or less.
[0050] The inductor 1 of such a structure can improve the DC superposition characteristics by using soft magnetic materials for magnetic particles, and is therefore used as an electronic component of a circuit where a large current flows, a DC-DC converter circuit, a choke coil of a power supply circuit, and is also used for electronic components of electronic equipment such as personal computers, DVD players, digital cameras, TVs, mobile phones, smart phones, automotive electronics, and medical / industrial machinery. However, the use of the inductor 1 is not limited to this, and for example, it can also be used in a tuning circuit, a filter circuit, a rectifier smoothing circuit, etc.
[0051] (Overview of Inductor Manufacturing Process)
[0052] Figure 4 It is a schematic diagram of the manufacturing process of the inductor 1.
[0053] As shown in the figure, the manufacturing process of the inductor 1 includes a coil conductor forming step, a preliminary molded body forming step, a green body molding / hardening step, a green body polishing step, and an external electrode forming step.
[0054] The coil conductor forming step is a step of forming the coil conductor 20 from a conductive wire. In this step, the coil conductor 20 is formed into a shape having the above-mentioned winding portion 22 and the lead portion 23 by winding the conductive wire using a winding method called "α winding". α winding refers to a state in which the conductive wire is wound in two stages in a spiral shape so that the lead portion 23 where the winding of the conductive wire, which functions as a conductor, starts and ends is located on the outer periphery. The number of turns of the coil conductor 20 is not particularly limited.
[0055] The preliminary molded body forming step is a step of forming a preliminary molded body called a flat plate.
[0056] The preformed body is formed into a solid state that is easy to handle by pressurizing the above-mentioned mixed powder serving as the material of the blank 2. In the present embodiment, two types of flat plates are formed: a first flat plate of an appropriate shape (e.g., E-type, T-type, etc.) for configuring the coil conductor 20, and a second flat plate of an appropriate shape (e.g., I-type, plate-shaped, etc.) sandwiching the coil conductor 20 between the first flat plate.
[0057] The green body forming / curing step is to place the first flat plate, the coil conductor, and the second flat plate in a forming mold, and pressurize the first flat plate and the second flat plate in the overlapping direction while heating, so that these structures are cured, and the first flat plate, the coil conductor, and the second flat plate are integrated. Thus, the green body 2 in which the coil conductor 20 is enclosed in the core 30 is formed. In addition, the green body 2 obtained by this step can also be roller-polished in order to remove burrs generated on the green body 2 or chamfer the corners of the green body 2.
[0058] The blank grinding process is a process of grinding the side surface 16 of the blank 2 and adjusting the width W of the blank 2. In the blank grinding process, the blank 2 is held by a plate-shaped member called a holding plate and clamped from above and below by the upper grinding wheel and the lower grinding wheel of the grinder. In this state, the side surface of the blank 2 is ground by operating the grinder to rotate the upper grinding wheel and the lower grinding wheel. Through the blank grinding process, the first side gap WSG, which is the sum of the width dimensions WSG1 and WSG2 described later, is less than 0.14 mm.
[0059] The external electrode forming step is a step of forming the external electrode 4 on the base body 2 , and includes a base body protective layer forming step, a surface treatment step, and a plating layer forming step.
[0060] The green body protective layer forming step is a step of coating the entire surface of the green body 2 with an insulating resin.
[0061] The surface treatment process is a process of modifying the surface of the predetermined electrode position on the surface of the core 30 by irradiating the predetermined electrode position with a laser. Here, the predetermined electrode position refers to the range of the surface of the core 30 where the external electrode 4 is to be formed, including the portion where the external electrode connection area 24 is exposed. Specifically, by irradiating the laser, the blank protective layer on the surface of the blank 2 and the covering layer of the external electrode connection area 24 of the coil conductor 20 are removed in the range of the predetermined electrode position, and the resin on the surface of the core 30 is removed, and the insulating film on the surface of the magnetic particles exposed from the core 30 is removed. As a result, the exposed area of the metal of the magnetic particles per unit area of the surface of the core 30 is increased compared with other surface portions of the core 30 in the portion of the predetermined electrode position on the surface of the core 30. In addition, after irradiating the laser, a cleaning process (such as etching process) for cleaning the surface of the predetermined electrode position may also be performed.
[0062] In the plating forming step, copper plating is formed at the electrode planned position to be irradiated with laser light by barrel plating copper on the surface of the core 30. Alternatively, the plating may be formed by further providing a Ni plating layer and a Sn plating layer on the copper plating layer.
[0063] The inductor 1 of the present embodiment will be described in further detail below. After describing the evaluation index of the characteristics of the inductor 1 and various parameters that affect the evaluation index, the preferred ranges of the various parameters will be described.
[0064] (Evaluation index of inductor characteristics)
[0065] As performance that is important in the inductor 1, in addition to inductance, the DC superposition rated current (hereinafter referred to as Isat) and the DC resistance (hereinafter referred to as Rdc) can also be cited. Isat is the current value when the inductance of the inductor 1 decreases by a specified proportion from the initial value due to magnetic saturation. In the present embodiment, it is the current value when it decreases by 30% from the initial value. Rdc is the resistance value when a DC current flows through the inductor 1. Generally speaking, the larger Isat is and the smaller Rdc is, the better the characteristics of the inductor 1 are. Therefore, in the present embodiment, the larger Isat / Rdc obtained by dividing Isat by Rdc is, the better the characteristics of the inductor 1 are evaluated.
[0066] (Parameter description)
[0067] In the inductor 1 , main parameters that affect Isat / Rdc include the total area S1 , the outer peripheral area S4 , the inner peripheral area S3 , the first side gap WSG , and the second side gap LSG . These parameters will be described below.
[0068] The total area S1 is the area of the main surface, that is, the area of either the upper surface 12 or the bottom surface 10. In addition, since the upper surface 12 and the bottom surface 10 are roughly rectangular shapes having sides along the DW direction and the DL direction, the total area S1 can also be calculated as the product of the width W of the blank 2 and the length L of the blank 2.
[0069] Figure 5 1 is a schematic diagram showing the blank 2 viewed from a direction perpendicular to the upper surface 12. Figure 5 The perspective view can be obtained by, for example, photographing with X-rays.
[0070] In this embodiment, since the blank 2 is a substantially rectangular parallelepiped, Figure 5As shown, the area inside the outer edge 2a of the blank 2 when viewed from a direction perpendicular to the upper surface 12 is substantially consistent with the area of the upper surface 12 and the bottom surface 10. Therefore, the area inside the outer edge 2a of the blank 2 when viewed from a direction perpendicular to the upper surface 12 may also be used as the total area S1.
[0071] The outer peripheral side area S4 is the area of the area between the outer periphery 22c of the winding portion 22 and the outer edge 2a of the blank 2 when the blank 2 is seen through from the direction perpendicular to the upper surface 12. The outer periphery 22c of the winding portion 22 refers to the outer edge of the conductor on the outermost peripheral side of the winding portion 22 when the two winding regions 22a and 22b are combined, as seen through from the direction perpendicular to the upper surface 12. That is, the outer periphery 22c may be composed of both the outer edge of the conductor on the outermost peripheral side of the winding region 22a and the outer edge of the conductor on the outermost peripheral side of the winding region 22b.
[0072] The inner circumference area S3 is the area of the inner side of the inner circumference 22d of the winding portion 22 when the base body 2 is seen through from the direction perpendicular to the upper surface 12. The inner circumference 22d of the winding portion 22 refers to the inner edge of the conductor on the innermost circumference of the winding portion 22 when the two winding regions 22a and 22b are combined, as seen through from the direction perpendicular to the upper surface 12. That is, the inner circumference 22d may be composed of both the inner edge of the conductor on the innermost circumference of the winding region 22a and the inner edge of the conductor on the innermost circumference of the winding region 22b.
[0073] The outer circumferential side area S4 and the inner circumferential side area S3 can be obtained by, for example, photographing the blank 2 with X-rays in a direction perpendicular to the upper surface 12, and measuring the area based on the obtained image, so that each measured value can be obtained. In addition, as described later, the outer circumferential side area S4 and the inner circumferential side area S3 are required to obtain the value S2 of the formula (1) described later. Since the value S2 is the value obtained by dividing the outer circumferential side area S4 by the inner circumferential side area S3, it is not necessary to respectively obtain the values of the outer circumferential side area S4 and the inner circumferential side area S3 in order to calculate the value S2. Therefore, it is also possible to calculate the ratio of the area equivalent to the outer circumferential side area S4 to the area equivalent to the inner circumferential side area S3 based on the image obtained by the above-mentioned X-ray photography, and directly obtain the value S2.
[0074] The first side gap WSG is the sum of the width dimensions WSG1 and WSG2 of the two first side gap portions 30a and 30b formed between the outer periphery 22c of the winding portion 22 and the two side surfaces 16 of the blank 2. The first side gap portions 30a and 30b are respectively a part of the core 30. In addition, the width dimensions WSG1 and WSG2 are both dimensions of the first side gap portions 30a and 30b in the DW direction. Specifically, the width dimension WSG1 of the first side gap portion 30a is the minimum value of the interval in the DW direction between the outer periphery 22c of the winding portion 22 and one side surface 16 when the blank 2 is seen through from a direction perpendicular to the upper surface 12. Similarly, specifically, the width dimension WSG2 of the first side gap portion 30b is the minimum value of the interval in the DW direction between the outer periphery 22c of the winding portion 22 and the other side surface 16 when the blank 2 is seen through from a direction perpendicular to the upper surface 12.
[0075] In addition, for example, Figure 5 As shown, the width dimensions WSG1 and WSG2 may also be the measured values of the interval between the outer periphery 22c of the winding portion 22 and the two side surfaces 16 on the imaginary line L1 when the blank 2 is seen through from a direction perpendicular to the upper surface 12. The imaginary line L1 is an imaginary straight line that passes through the reel Q of the winding portion 22 and extends in the DW direction when the blank 2 is seen through from a direction perpendicular to the upper surface 12. By measuring the width dimensions WSG1 and WSG2 in this way, the width dimensions WSG1 and WSG2 can be made sufficiently close to the minimum value of the interval between the outer periphery 22c of the winding portion 22 and the side surface 16 in the DW direction when the blank 2 is seen through from a direction perpendicular to the upper surface 12. In addition, the position of the reel Q when the blank 2 is seen through from a direction perpendicular to the upper surface 12 may also be, for example, the center of the largest inscribed circle relative to the inner periphery 22d of the winding portion 22. In addition, the imaginary line L1 may also be arranged at the center of the blank 2 in the DL direction.
[0076] The second side gap LSG is the sum of the length dimensions LSG1 and LSG2 of the two second side gap portions 30c and 30d formed between the outer periphery 22c of the winding portion 22 and the two end faces 14 of the blank 2. The second side gap portions 30c and 30d are respectively a part of the core 30. In addition, the length dimensions LSG1 and LSG2 are both dimensions of the second side gap portions 30c and 30d in the DL direction. Specifically, the length dimension LSG1 of the second side gap portion 30c is the minimum value of the interval in the DL direction between the outer periphery 22c of the winding portion 22 and one end face 14 when the blank 2 is seen through from a direction perpendicular to the upper surface 12. Similarly, specifically, the length dimension LSG2 of the second side gap portion 30d is the minimum value of the interval in the DL direction between the outer periphery 22c of the winding portion 22 and the other end face 14 when the blank 2 is seen through from a direction perpendicular to the upper surface 12. In addition, in Figure 5In the embodiment, there is a lead-out portion 23 extending from the outer periphery 22c of the winding portion 22 toward the end face 14 of the blank, but the portion where the lead-out portion 23 is connected to the winding portion 22, i.e., the portion where the surface on the winding axis Q side of the outermost conductor begins to separate from the inner conductor is removed from the outer periphery 22c of the winding portion.
[0077] In addition, for example, Figure 5 As shown, the length dimensions LSG1 and LSG2 may also be the measured values of the interval between the outer periphery 22c of the winding portion 22 and the two end faces 14 on the imaginary line L2 when the blank 2 is seen through from the direction perpendicular to the upper surface 12. The imaginary line L2 is an imaginary straight line that passes through the winding axis Q of the winding portion 22 and extends in the DL direction when the blank 2 is seen through from the direction perpendicular to the upper surface 12. By measuring the length dimensions LSG1 and LSG2 in this way, the length dimensions LSG1 and LSG2 can be made to be sufficiently close to the minimum value of the interval between the outer periphery 22c of the winding portion 22 and the side surface 14 in the DL direction when the blank 2 is seen through from the direction perpendicular to the upper surface 12. In addition, the imaginary line L2 may also be arranged at the center of the blank 2 in the DW direction.
[0078] (Preferred range of parameters)
[0079] As a result of the following examples carried out by the inventors, it was found that the preferred range of the value K obtained by the following formula (1) for increasing Isat / Rdc is 70 to 110. In addition, it was found that the more preferred range of the value K is 80 to 100.
[0080] K=S1 / (WSG×LSG)×(S4 / S3)
[0081] =(S1 / SG)×(S4 / S3)
[0082] =B×S2 (1)
[0083] In the present embodiment, the value K is greater than or equal to 70 and less than or equal to 110. Therefore, Isat / Rdc of the inductor 1 can be increased, and the inductor 1 having good characteristics can be obtained.
[0084] [Example]
[0085] The inventors conducted experiments to verify the relationship between the various parameters and the characteristics of the inductor. In the embodiment, the inventors produced a green body 2, and changed various parameters in simulation based on the produced green body 2 to calculate the value K. In addition, the inventors calculated Isat / Rdc for each calculated value K to obtain a preferred range of the value K. The details are described below.
[0086] (Preparation of Samples)
[0087] First, the inventor prepared a blank 2 for simulation. The inventor used a material made by mixing Fe-Si-Cr alloy powder as the first magnetic particle and carbonyl iron powder as the second magnetic particle as the metal magnetic powder in the mixed powder as the material of the core 30. According to the measurement results of the particle size distribution meter, the average particle size of the first magnetic particle of the metal magnetic powder of the embodiment is 25.3μm, and the average particle size of the second magnetic particle is 1.7μm. In addition, the resin of the embodiment contains bisphenol A type epoxy resin and rubber modified epoxy resin, which occupy 2.7wt% in the mixed powder. According to the inventor's measurement, the relative magnetic permeability of the mixed powder is 34 and the saturation magnetic flux density is 1.36T. In addition, the relative magnetic permeability is measured using a BH analyzer and an impedance material analyzer using a high-frequency signal with a frequency of 1MHz. In addition, for the saturation magnetic flux density, the inductance change during overlap is measured using an LCR meter and a DC power supply, and the BH data is inversely calculated, and the value of magnetic flux saturation is used as the saturation magnetic flux density of the mixed powder.
[0088] In the example, the inventors used a rectangular wire with a cross-sectional dimension of 0.128 mm in length and 0.083 mm in width to produce a coil conductor 20. The coil conductor 20 has a winding portion 22 and a lead portion 23 formed by winding in two stages, similarly to the first embodiment.
[0089] In the embodiment, the inventors used the core 30 and the coil conductor 20 described above to produce a blank 2. During compression molding, the coil conductor 20 was arranged in an E-type preformed body made by mixing the same metal magnetic powder and resin as the core 30 of the embodiment. In addition, the coil conductor 20 was arranged in the mold in a state of being clamped between the E-type preformed body and the I-type preformed body made of the same material as the E-type preformed body. In this state, the E-type preformed body, the coil conductor 20, and the I-type preformed body were hot-compressed to form the blank 2. In addition, at this time, the coil conductor 20 is in a posture in which the winding axis Q of the winding portion 22 is approximately vertical relative to the bottom surface 10 which is the mounting surface of the blank 2.
[0090] Thus, a blank 2 having a length L of 1.52 mm in the longitudinal direction DL, a width W of 1.35 mm in the width direction DW, and a thickness T of 0.57 mm in the thickness direction DT was produced.
[0091] (simulation)
[0092] Figure 6 It is a graph showing various parameters during simulation and the calculated value K. In addition, Figure 6 The characters of the parameters correspond to the characters of the parameters described in Embodiment 1. In addition, the inner diameter R is the value of the curvature radius of the curved portion of the inner circumference 22 d of the winding portion 22 .
[0093] The inventors simulated the shapes of various parts of the obtained green body 2 and calculated the value K of the green body 2 with a first side gap WSG of 0.1 mm, a second side gap LSG of 0.2 mm, and an inner diameter R of the coil conductor 20 of 0.25 mm. The calculated value K was 63.4.
[0094] Afterwards, the inventors calculated the value K in simulation for each mode in which the inductance value becomes 0.31 μH by changing the cross-sectional dimensions of the rectangular wire, the size of the inner diameter R, the size of the first side gap WSG, and the size of the second side gap LSG. At this time, the outer dimensions of the blank 2 are fixed at 1.52 mm in length L, 1.35 mm in width W, and 0.57 mm in thickness T. As a result, Figure 6 As shown, for the combination of parameters of the 12 patterns in total, a value K in the range of 59.8 or more and 112.5 or less is obtained.
[0095] In addition, the present invention is not limited to such simulations. In actual manufacturing, the first side gap WSG and the second side gap LSG can be adjusted by changing the size of the space in the mold. In addition, the size of the first side gap WSG and the second side gap LSG can be adjusted by making the size of the space in the mold larger than the final size of the blank 2 and grinding the core 30 after compression molding.
[0096] The inventor further Figure 6 The changes in Isat / Rdc corresponding to the value of K were simulated.
[0097] Figure 7 This is a graph showing the relationship between the value K and Isat / Rdc in the simulation. Figure 8 : is a graph showing the relationship between the value K and Isat / Rdc in the simulation. Figure 8 The curve is Figure 7 The various results of the simulations shown are interpolated curves.
[0098] like Figure 7 and Figure 8 As shown in the figure, among the values of K simulated, the maximum Isat / Rdc is when the value of K is 93.2, and the Isat / Rdc at this time is 0.2629A / mΩ. Figure 7 As shown, Isat / Rdc has a peak value, and as the value K increases or decreases from the value at the peak value, Isat / Rdc tends to decrease.
[0099] In addition, if Figure 7 and Figure 8As shown, in the second simulation of the embodiment, Isat / Rdc in the range of value K being 70 to 110 changes to 90% or more of the maximum value of Isat / Rdc. Also, Isat / Rdc in the range of value K being 80 to 100 changes to 95% or more of the maximum value of Isat / Rdc.
[0100] Therefore, according to the examples, it was found that if the measurement accuracy of each parameter in the actual object is also taken into account, the preferred range of the value K is 70 to 110. In addition, according to the examples, it was found that the more preferred range of the value K is 80 to 100.
[0101] Although the reason for obtaining such an effect is not clear, it is considered that this is because a different design concept from that of conventional products having a device size larger than the 1412 size (1.4 mm×1.2 mm) is required.
[0102] In addition, Isat / Rdc has a value K Figure 7 The reason for the peak values shown is considered to be that there is a preferred range for increasing Isat / Rdc for each of the value B and the value S2 used in the above-mentioned equation (1).
[0103] When the value S2 is large, the outer peripheral area S4 is large and the inner peripheral area S3 is small. In this case, since the outer peripheral area S4 is large, the diameter of the outer periphery 22c is small, the length of the wire forming the coil conductor 20 is easy to be shortened, and Rdc is easy to be reduced. On the other hand, since the inner peripheral area S3 is small, magnetic saturation is easy to occur, and Isat is easy to be reduced.
[0104] The case where the value S2 is small is the case where the outer peripheral side area S4 is small and the inner peripheral side area S3 is large. In this case, since the outer peripheral side area S4 is small, the diameter of the outer periphery 22c is large, the length of the wire forming the coil conductor 20 is easy to increase, and Rdc is easy to increase. On the other hand, since the inner peripheral side area S3 is large, it is difficult to produce magnetic saturation, and Isat is easy to increase.
[0105] Thus, when the value S2 is large, both Rdc and Isat tend to decrease, and when the value S2 is small, both Rdc and Isat tend to increase. Therefore, it is considered that Isat / Rdc does not increase or decrease monotonically with respect to the value S2, and there is a preferred range of the value S2 for increasing Isat / Rdc.
[0106] If the total area S1 is regarded as the product of the width W and the length L, the value B can be transformed as shown in the following formula (2).
[0107] B=S1 / SG
[0108] =(W×L) / (WSG×LSG)
[0109] =(W / WSG)×(L / LSG) (2)
[0110] That is, the value B is considered to be the product of the inverse of the ratio WSG / W of the first side gap WSG to the width W and the inverse of the ratio LSG / L of the second side gap LSG to the length L.
[0111] Therefore, the case where the value B is large is the case where the ratios WSG / W and LSG / L are small. In this case, it means that when viewed from a direction perpendicular to the upper surface 12, the outer periphery 22c of the winding portion 22 is located close to the side surface 16 and the end surface 14 of the blank 2. That is, the length of the wire constituting the coil conductor 20 is easy to increase, and Rdc is easy to increase. In addition, since the diameter of the inner periphery 22d of the winding portion 22 is easy to increase, it is difficult to achieve magnetic saturation, and Isat is easy to increase.
[0112] In addition, the case where the value B is small is the case where each ratio WSG / W and LSG / L is large. In this case, it means that when viewed from a direction perpendicular to the upper surface 12, the outer periphery 22c of the winding portion 22 is located away from the side surface 16 and the end surface 14 of the blank 2. That is, the length of the wire constituting the coil conductor 20 is easy to shorten, and Rdc is easy to become small. In addition, since the diameter of the inner periphery 22d of the winding portion 22 is easy to become small, it is easy to be magnetically saturated, and Isat is easy to become small.
[0113] As described above, when the value B is large, both Rdc and Isat tend to increase, and when the value B is small, both Rdc and Isat tend to decrease. Therefore, it is considered that Isat / Rdc does not increase or decrease monotonically with respect to the value B, and there is a range of values of B that are preferred for increasing Isat / Rdc.
[0114] Thus, it is considered that the value B and the value S2 each have a preferred range in terms of increasing Isat / Rdc. Therefore, it is considered that the value K, which is the product of the value B and the value S2, also has a preferred range in terms of increasing Isat / Rdc.
[0115] [Implementation Method 2]
[0116] Next, use Fig. 9 and Fig.10 Embodiment 2 will be described. In the following, only the points different from Embodiment 1 will be described, and the same description will be omitted.
[0117] Fig. 9 This is a perspective view of the blank 102 according to the second embodiment. Fig. 9 It is a schematic diagram showing the blank 102 as seen from a direction perpendicular to the upper surface 12 .
[0118] In the blank 102 of the second embodiment, unlike the blank 2 of the first embodiment, the cross-section 123a of the wire constituting the two lead-out portions 123 of the coil conductor 20 is exposed from the two end faces 14. More specifically, the cross-section 123a of the wire constituting the lead-out portion 123 is substantially coplanar with the two end faces 14 of the blank 102. In other words, the cross-section 123a of the wire constituting the lead-out portion 123 is substantially on the same plane as the end face 14 of the blank 102. For example, in the blank grinding step, by cutting the two end faces 14 of the blank 102 together with the lead-out portion 123 in the DL direction, the cross-section 123a of the wire constituting the lead-out portion 123 is exposed from the end face 14 of the blank 102 and is substantially coplanar with the end face 14. Furthermore, a cross section 123 a of a lead wire constituting the lead portion 123 exposed from the end surface 14 of the base body 102 is connected to the external electrode 4 in the external electrode forming step.
[0119] In this way, by cutting the end face 14 of the blank 102 so that the cross section 123a of the wire constituting the lead portion 123 is exposed from the end face 14 of the blank 102, the length dimensions LSG1 and LSG2 of the second side gaps 30c and 30d can be easily adjusted. Therefore, the value K calculated by the above formula (1) can be easily adjusted to be greater than 70 and less than 110.
[0120] [Implementation method 3]
[0121] Next, use Fig.11 and Fig.12 , Embodiment 3 is described. In addition, only the points different from Embodiment 1 and Embodiment 2 are described below, and the same description is omitted.
[0122] Fig.11 This is a perspective view of the blank 202 according to the third embodiment. Fig.12 It is a schematic diagram showing the blank 202 viewed from the bottom surface 10 side.
[0123] In the green body 202 of the third embodiment, unlike the first and second embodiments, the two lead portions 223 of the coil conductor 20 are bent toward the bottom surface 10, and the lead portions 223 are exposed from the bottom surface 10. More specifically, the surface 223a of the wire constituting the lead portion 223 is exposed from the bottom surface 10 of the green body 202. In addition, the surface 223a of the wire constituting the lead portion 223 exposed from the bottom surface 10 of the green body 202 is connected to the external electrode 4 in the external electrode forming step.
[0124] In this way, by exposing the surface 223a of the wire constituting the lead portion 223 from the bottom surface 10 of the base body 202, the lead portion 223 and the external electrode 4 can be connected even if the lead portion 223 is not exposed from the end surface 14 of the base body 202. Therefore, it is not necessary to expose the lead portion 223 from the end surface 14 of the base body 202, and the degree of freedom of adjustment of the length dimensions LSG1 and LSG2 of the second side gaps 30c and 30d can be increased. Therefore, it is easy to adjust the value K calculated by the above formula (1) to 70 or more and 110 or less.
[0125] [Other embodiments]
[0126] In the above embodiment, the external electrode 4 is described as an L-shaped electrode formed across the end surface 14 and the bottom surface 10 of the body 2, 102, 202, but this is an example. The external electrode 4 is not limited to the L-shaped electrode, and may be a structure formed across the end surface 14 of the body 2, 102, 202 and the bottom surface 10 adjacent to each end surface 14, the upper surface 12, and the two side surfaces 16. In this case, the surface 223a of the wire constituting the lead portion 223 described in the third embodiment may be exposed from the upper surface 12 instead of the bottom surface 10 of the body 202.
[0127] In the above embodiment, two first side gaps 30a and 30b are formed between the winding portion 22 and the two side faces 16, but this is an example. For example, the outer periphery 22c of the winding portion 22 may be exposed from one side face 16, and only one of the first side gaps 30a and 30b may be formed. In this case, the first side gap WSG is consistent with one of the width dimensions WSG1 and WSG2. Similarly, the winding portion 22 may be exposed from one side of the end face 14, and only one of the second side gaps 30c and 30d may be formed between the winding portion 22 and the two end faces 14, and the second side gap LSG is consistent with one of the length dimensions LSG1 and LSG2.
[0128] All the above-mentioned embodiments and modifications are contents of one mode of the present invention, and can be arbitrarily modified and applied within the scope not departing from the gist of the present invention. In addition, arbitrary elements of the above-mentioned embodiments can also be combined to form a new embodiment.
[0129] In addition, the horizontal, orthogonal and vertical directions, various numerical values, shapes and materials in the above-mentioned embodiments also include ranges having the same effects as these directions, numerical values, shapes and materials (so-called equivalent ranges) unless otherwise specified.
[0130] [Structure supported by the above-mentioned embodiment]
[0131] The above-mentioned embodiment supports the following structure.
[0132] (Structure 1) An inductor, comprising: a coil having a winding portion and a pair of lead portions, wherein the winding portion is formed by winding a rectangular wire, and the pair of lead portions are led out from the winding portion; a blank containing magnetic powder and resin, and having the coil built therein; and external terminals formed on the surface of the blank and connected to the lead portions, the blank having: a main surface intersecting with the winding axis of the coil and having a rectangular shape with sides along a first direction and a second direction; a pair of first surfaces adjacent to the main surface and along the first direction; a pair of second surfaces adjacent to the main surface and along the second direction; first side gap portions formed respectively on the winding portions. between the outer periphery of the part and the above-mentioned pair of first surfaces; and the second side gap portions are respectively formed between the above-mentioned outer periphery and the above-mentioned pair of second surfaces, when the area of the above-mentioned main surface is set to S1, the total size of the above-mentioned second direction of each of the above-mentioned first side gap portions is set to WSG, the total size of the above-mentioned second side gap portions in the first direction is set to LSG, the area of the inner side of the inner periphery of the above-mentioned winding portion when viewed from a direction perpendicular to the above-mentioned main surface is set to S3, the area between the above-mentioned outer periphery and the outer edge of the above-mentioned blank is set to S4, and SG is set to the value obtained by the following formula (A), K obtained by the following formula (B) is greater than 70 and less than 110,
[0133] SG=WSG×LSG (A)
[0134] K = (S1 / SG) x (S4 / S3) (B).
[0135] According to the inductor of Structure 1, Isat / Rdc can be improved. Therefore, an inductor having good characteristics can be provided.
[0136] (Structure 2) In the inductor according to Structure 1, a cross section of the conductive wire constituting the lead portion is exposed on the second surface, and the cross section is flush with the second surface.
[0137] According to the inductor of Structure 2, the dimension of the second side gap portion in the first direction can be easily adjusted, and K can be easily adjusted to be greater than or equal to 70 and less than or equal to 110. Therefore, an inductor having good characteristics can be easily provided.
[0138] (Structure 3) In the inductor according to Structure 1 or 2, a surface of the conductive wire constituting the lead portion is exposed from the main surface.
[0139] According to the inductor of Structure 3, the degree of freedom of the dimension of the second side gap portion in the first direction increases, and K can be easily adjusted to be greater than or equal to 70 and less than or equal to 110. Therefore, an inductor having good characteristics can be easily provided.
Claims
1. An inductor comprising: The coil has a winding portion and a pair of lead portions, wherein The winding portion is formed by winding a rectangular wire, and the pair of lead portions are led out from the winding portion; A blank body, comprising magnetic powder and resin, and having the coil built therein; The external terminal is formed on the surface of the above-mentioned blank and connected to the above-mentioned lead portion. The above-mentioned blank has: A main surface intersecting with the winding axis of the coil and having a rectangular shape having sides along the first direction and the second direction; a pair of first surfaces, adjacent to the main surface and along the first direction; a pair of second surfaces, adjacent to the main surface and along the second direction; first side gap portions, each formed between the outer periphery of the winding portion and the pair of first surfaces; The second side gaps are formed between the outer periphery and the pair of second surfaces, respectively. When the area of the main surface is set to S1, The sum of the dimensions of the first side gaps in the second direction is denoted as WSG. The total of the dimensions of the second side gaps in the first direction is LSG. The area inside the inner periphery of the winding portion when viewed from a direction perpendicular to the main surface is defined as S3, and the area between the outer periphery and the outer edge of the blank is defined as S4. When SG is set to the value obtained by the following formula (A), K calculated by the following formula (B) is 70 or more and 110 or less, SG=WSG×LSG(A) K = (S1 / SG) x (S4 / S3) (B).
2. The inductor according to claim 1, wherein The cross section of the wire constituting the lead-out portion is exposed on the second surface. The cross section is coplanar with the second surface.
3. The inductor according to claim 1 or 2, wherein: A surface of the lead forming the lead portion is exposed from the main surface.
Citation Information
Patent Citations
Method of manufacturing surface mounting inductor and the surface mounting inductor
JP2010245473A