Integrally-formed inductor capable of enhancing electrode stability
By designing the matching structure of the air-core coil and the magnet in the integrated molded inductor, combined with the molding technology of flat electrodes and filler-type conductive adhesives, the problems of unstable electrode structure and reduced molding size are solved, achieving higher electrode adhesion and signal. Stability, suitable for high-density circuit board layout.
Patent Information
- Application Number
- CN202411093360.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-01
AI Technical Summary
The electrode structure of the existing one-piece inductor is unstable, which causes the concentration of mechanical stress, affects the electrode adhesion, increases the problems of poor contact and signal attenuation, and it is difficult to reduce the molding size to adapt to the high-density circuit board layout.
Design an integrated inductor that enhances the stability of the electrode. Through the cooperation of the air-core coil and the magnet, the symmetrical structure of the base and the columnar protrusion is used, combined with the flat electrode and the filler type conductive adhesive, and is bent and hot-pressed twice. , ensure the positioning and connection stability of the electrode, and improve the mechanical strength and electrical insulation performance of the magnet by optimizing the particle size of the magnetic powder and the additive ratio.
It effectively reduces the rate of electrode defective products, improves the mechanical strength and adhesion of the electrode, reduces poor contacts, enhances the electrical performance and signal stability of the inductor, and at the same time achieves smaller molding size and higher density layout adaptability. .
Smart Images

Figure CN118737666A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of integrated molded inductor manufacturing, and in particular relates to an integrated molded inductor with enhanced electrode stability. Background Art
[0002] The one-piece molded inductor is formed by pressing the coil, electrode sheet and powder together. With the continuous advancement of technology, the trend of electronic products is to develop thinner and smaller. The components such as resistors, capacitors and inductors installed on the printed integrated circuits of electronic products also need to reduce their molding size. The commonly used pressed inductors include coils, magnetic core bodies and lead frames. The two electrode pins of the lead frame are welded to the two ends of the coil and embedded in the magnetic body. The two electrode pin terminals extend out of the body and form electrodes on the surface of the body. The specific structure of the inductor after molding is as follows Fig.11 shown.
[0003] At present, inductors and circuit boards are installed using SMT surface mounting technology. Since the electrodes are located on the left and right sides, the overall size of the inductor cannot be further reduced. Moreover, since the electrodes are located on both sides, the mechanical stress is concentrated in the solder joint area, which is prone to stress concentration problems during welding and subsequent use, thereby affecting the stability of the electrode. The electrode stability performance refers to the adhesion between the electrode surface and the product body. When the electrode adhesion is poor, it will lead to poor contact, thereby increasing the contact resistance and affecting the electrical performance of the inductor. Poor contact will lead to unstable signal transmission, signal attenuation or increased noise.
[0004] To address the above problems, the currently adopted structural design is to design the electrodes on the bottom of the inductor to reduce the lateral size and thus adapt to higher density circuit board layouts. For example, the inductor disclosed in announcement number CN112151232B has electrodes attached to its bottom and symmetrically arranged.
[0005] However, the connection between the electrode and the magnet in the above-mentioned inductor is unstable. In particular, the pin wire of the copper ring is twisted and then bent to form the electrode. The deformation caused by the twisting may cause cracks. In addition, the mechanical strength of the magnet itself of the existing inductor is not high. In view of the existing problems, the applicant has developed a new integrated inductor that can ensure the stability of the electrode while ensuring the normal operation of the circuit. Summary of the invention
[0006] The purpose of the present invention is to provide an integrated inductor with enhanced electrode stability in order to solve the problem that the electrode structure of the existing integrated inductor is unstable and affects the reduction of the inductor volume.
[0007] The present invention is achieved through the following technical solutions: An integrated inductor for enhancing electrode stability comprises a hollow coil and a magnet, wherein both ends of the hollow coil are lead wires, and the magnet is obtained by cold pressing magnetic powder, and the magnet comprises a base and a columnar protrusion. One side of the base is symmetrically provided with an empty groove relative to the columnar protrusion, and the bottom surface of the base is provided with two grooves. The hollow coil is sleeved outside the columnar protrusion, and the lead wire is stripped of paint and flattened to obtain a connecting wire. The end of the connecting wire is connected to a flat electrode on the top surface of the base, and the flat electrode is bent twice and passed through the empty slot and then clamped in the groove to obtain an inductor intermediate; the inductor intermediate is placed in a mold, filled with magnetic powder material 2, and hot pressed to obtain an inductor; The particle size of the magnetic powder material 1 is 40-60 μm, the content of the epoxy insulating resin in the magnetic powder material 1 is 2.8-3.4% of the total weight of the magnetic powder material 1, the cold pressing temperature of the magnet is 35-45° C., and the pressure is 120-140 MPa; The particle size of the magnetic powder is 2-6 μm, the content of epoxy insulating resin in the magnetic powder is 0.8-1.2% of the total weight of the magnetic powder, the hot pressing temperature is 200-220° C., the pressure is 68-70 MPa, and the pressure holding time is 140-160 s.
[0008] The present invention is further configured as follows: the inner ring structure of the hollow coil matches the columnar protrusion, and the hollow coil is one layer or multiple layers.
[0009] The present invention is further configured as follows: a connection groove is formed on the top surface of the base on the path where the pin line passes, and the connection line is pressed into the connection groove and fixedly connected with the flat electrode.
[0010] The present invention is further configured as follows: the end of the connecting wire is bonded to the flat electrode by a filler-type conductive adhesive. The filler-type conductive adhesive comprises the following raw materials in parts by weight: 65-75 parts of epoxy resin, 4.6-5.6 parts of gold powder, 2-3 parts of graphite powder, 6-10 parts of solvent, and 1-2 parts of thixotropic agent.
[0011] The present invention is further configured such that: the height of the columnar protrusion is 1-1.05 times the axial height of the hollow coil.
[0012] The present invention is further configured as follows: the hot pressing mold of the magnetic powder second is preheated to 120-140°C before hot pressing.
[0013] The present invention is further configured as follows: the magnetic powder material 1 and the magnetic powder material 2 are both composed of metal powder, a binder and an additive, wherein the binder is epoxy resin, the metal powder is iron silicon chromium powder, and the additive is composed of SKF LGEM 2 and tungsten diselenide.
[0014] The present invention is further configured as follows: the content of the additive in the magnetic powder material 1 is 0.4-0.6% of the total weight of the magnetic powder material 1, and the weight ratio of SKF LGEM 2 and tungsten diselenide in the additive is 1:3-5; The content of the additive in the magnetic powder material 2 is 0.1-0.2% of the total weight of the magnetic powder material 1, and the weight ratio of SKFLGEM 2 to tungsten diselenide in the additive is 2:1.
[0015] The present invention is further configured such that: the thickness of the flat electrode is 1.2-1.4 times the depth of the connecting groove.
[0016] Compared with the prior art, the present invention has the following advantages: Through the cooperation of the base and the columnar protrusion, the hollow coil can be effectively positioned to avoid the problem of uneven magnetic permeability caused by uneven particles inside the hollow coil; after the flat electrode and the connecting wire are connected and fixed on the side with the hollow coil, the flat electrode is bent twice and then hot-pressed to obtain a molded inductor, the damage to the hollow coil during the pressing process is reduced, the defective rate of the one-piece molded inductor is effectively reduced, and the high requirements for the yield rate of the molded inductor can be met; in addition, the molded inductor structure can be reduced according to actual needs, and the two flat electrodes can be effectively isolated; on the basis of the hollow coil being sleeved on the positioning base, the loss can be reduced while the molded inductor has good mechanical strength, the flat electrode and the connecting wire can be prevented from loosening during the pressing process, and the electrode stability is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1a It is a schematic diagram of the structure of an air-core coil; Figure 1b It is a schematic diagram of the structure after the pin wire ends of the hollow coil are flattened; Figure 2 It is a structural schematic diagram of the positioning base; Figure 3 It is a schematic diagram of the bottom surface structure of the positioning base; Figure 4 is a side view of the positioning base; Figure 5 It is a structural schematic diagram of a positioning base with a hollow coil; Figure 6 It is a schematic diagram of the structure of connecting wires to flat electrodes; Figure 7 It is a side view of the flat electrode connected with the connecting wire; Figure 8 It is a schematic diagram of the structure of the flat electrode when it is bent for the first time; Fig. 9 It is a schematic diagram of the structure of the flat electrode when it is bent for the second time; Fig.10 It is a schematic diagram of the structure of the formed inductor; Fig.11 It is a structural schematic diagram of the prior art. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with the accompanying drawings.
[0019] The following will be combined with the accompanying drawings of the embodiments of the present invention to clearly and completely describe the technical solutions of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] As shown in Figures 1-5, the inductor includes a hollow coil 2 and a magnet. Two electrodes are attached to the outer surface of the magnet. The internal structure of the magnet includes a base and a columnar protrusion vertically connected to the base. The magnet is a magnetic powder material and is formed in one piece by cold pressing.
[0021] The particle size of the magnetic powder material 1 is 40-60 μm, the content of epoxy insulating resin in the magnetic powder material 1 is 3.2% of the total weight of the magnetic powder material 1, and the content of additives is 0.5% of the total weight of the magnetic powder material 1; the weight ratio of SKF LGEM 2 and tungsten diselenide in the additive is 1:4; the cold pressing temperature of the magnet is 35° C. and the pressure is 130 MPa.
[0022] Optimize magnetic properties: Magnetic powder with a particle size of 40-60μm helps to form a uniform magnetic field and ensures that the magnet has good magnetic permeability and stable magnetic properties. The moderate particle size makes the powder easier to handle and shape during the pressing process.
[0023] The content of epoxy insulating resin is 3.2%, which ensures good electrical insulation performance and reduces the performance degradation of the magnet caused by electrical problems during operation.
[0024] SKF LGEM 2: acts as a lubricant, helping to improve the flow properties of powders and reduce friction during processing.
[0025] Tungsten diselenide: As one of the additives, it improves the thermal stability and wear resistance of the powder. The 1:4 ratio with SKF LGEM 2 optimizes the effect of the additive and improves the overall performance of the magnet.
[0026] Cold pressing process parameters: Temperature: The cold pressing temperature of 35°C is controlled within a relatively low range, ensuring that the powder will not experience excessive thermal expansion or structural deformation during the curing process, thus ensuring the molding accuracy.
[0027] Pressure: 130MPa pressure helps to evenly press the powder into shape, improving the density and overall magnetic properties of the magnet. High pressure can also reduce pores and defects, making the magnet more dense and stable.
[0028] The two ends of the hollow coil 2 form lead wires 2a, and the inner ring structure of the hollow coil 2 matches the columnar protrusion 13, that is, the hollow coil is sleeved outside the columnar protrusion, the hollow coil 2 has two layers, and the lead wires 2a are parallel to each other.
[0029] Two empty grooves are provided on one side wall of the base 1, and the two empty grooves are arranged relative to the two sides of the columnar protrusion. Two parallel grooves 12 are provided on the bottom surface of the base. The grooves are rectangular. The height of the columnar protrusion 13 is 1-1.05 times the axial height of the hollow coil 2. The design of this application is 1.05 times. The purpose is to avoid a large extrusion pressure on the hollow coil 2 during the hot pressing process, thereby reducing the damage of the paint film on the surface of the hollow coil 2.
[0030] The lead wire 2a is stripped of paint and flattened to obtain a connecting wire 2b, such as Figure 6-7 A connection groove 14 is provided on the top surface of the connection base 1 at the bottom of the lead wire 2a. The connection wire 2b is pressed into the connection groove 14 and fixedly connected to the flat electrode 3, and the two are bonded by a filler-type conductive adhesive.
[0031] The connection groove 14 provides a structured space, providing a stable positioning area for the connection wire and the electrode, and the filler-type conductive glue can fill this area, further enhancing the mechanical stability of the connection, avoiding poor contact caused by mechanical stress during use, and the thickness of the flat electrode is designed to be 1.2-1.4 times the depth of the connection groove, ensuring that the electrode is fully in contact with the connection wire and the base surface. This thickness design avoids poor contact, improves electrical conductivity, ensures stable electrical connection, and can ensure that the flat electrode is conveniently fixed to the circuit board after hot pressing.
[0032] The filler-type conductive adhesive includes the following raw materials in parts by weight: 70 parts of epoxy resin, 5 parts of gold powder, 2.5 parts of graphite fluoride, 0.4 parts of manganese acetylacetonate, 6 parts of acetone, 2 parts of ethylene glycol butyl ether, and 1.5 parts of LBCB-1 thixotropic lubricant; the conductive adhesive has stable conductivity and good high temperature resistance while ensuring strong bonding strength. The combination of gold powder, graphite fluoride and manganese acetylacetonate can effectively avoid electrolytic migration, thereby avoiding problems that affect current conductivity.
[0033] Electrolytic migration refers to the migration of electrons or ions in a conductive adhesive under the action of an electric field, which may cause metal ions to migrate from one place to another, resulting in a decrease in conductivity and may even cause an electrical short circuit.
[0034] The high conductivity and corrosion resistance of gold powder, the chemical stability of graphite fluoride, and the catalytic effect of manganese acetylacetonate work together to reduce the occurrence of electrolytic migration. Specifically: gold powder ensures the integrity of the conductive network and reduces the change in conductive properties caused by metal corrosion. Graphite fluoride provides chemical stability and reduces chemical reactions caused by friction due to its good lubricity. Manganese acetylacetonate reduces the risk of electrolytic migration by stabilizing the chemical environment of the glue.
[0035] The volume resistivity of the conductive adhesive produced by the use of the ratio is low (0.039Ω·cm), which means that it has good electrical conductivity. Even under aging conditions of 150°C, its resistivity does not change much (down to 0.034Ω·cm), ensuring stable current conductivity.
[0036] Moreover, the shear strength is 37MPa, which ensures a strong bond between the connecting wire and the electrode and enhances the overall mechanical stability and durability.
[0037] After being bent twice, the flat electrode 3 is clamped in the groove through the empty groove 11. Figure 8 The first bending body 32 shown in the figure is bent for the second time to obtain the following Fig. 9 The secondary bending body 33 shown in the figure has the flat electrode clamped in the groove to obtain an inductor intermediate body.
[0038] By bending twice, the flat electrode can be accurately stuck in the groove. The electrical connection problem caused by unstable electrode position is reduced. This forms a tight inductor intermediate body, thereby improving the reliability of the overall connection. Moreover, the bent electrode design can better adapt to the spatial layout of the inductor, which helps to achieve better layout and connection in a limited space, and improves the space utilization of the product.
[0039] like Fig.10 As shown in the figure, the preparation process of the molded inductor is as follows: the inductor intermediate is placed in a mold, filled with magnetic powder material 2, and hot pressed. The hot pressing temperature is 200°C, the pressure is 70MPa, and the pressure holding time is 150s. Before hot pressing, the molded inductor is preheated to 120°C, which can reduce the energy consumption during the hot pressing process and prevent the magnetic powder material 2 from being affected by the temperature and affecting the hot pressing structure.
[0040] The particle size of the magnetic powder material 2 is 2-6 μm, the content of epoxy insulating resin in the magnetic powder material 2 is 0.8% of the total weight of the magnetic powder material 2, the content of additives in the magnetic powder material 2 is 0.1% of the total weight of the magnetic powder material 1, and the weight ratio of SKF LGEM2 and tungsten diselenide in the additive is 2:1.
[0041] The outer layer of magnetic powder can increase the surface wear resistance of the magnet and prevent the external environment from corroding the magnet. Fine particles and additives such as SKF LGEM 2 and tungsten diselenide enhance the hardness and durability of the outer layer. The fine particle size and the ratio of additives optimize the molding process of the outer layer, making its surface smoother and more uniform, reducing defects and bubbles. This can improve the mechanical strength and stability of the magnet.
[0042] Because: electrode stability represents the adhesion between the electrode surface and the product body, and the thrust test reflects the corresponding relationship. The greater the adhesion, the greater the thrust.
[0043] The thrust test of the products produced according to the existing process and the products of this application is as follows.
[0044] When using a thrust gauge, the thrust gauge is required to apply force at an angle of 30 to 45 degrees to the material being tested, and the force must reach the specified standard at a uniform speed.
[0045] Serial number Improved forward thrust test (N) Improved thrust test (N) 1 166 201 2 175 207 3 190 218 4 198 223 5 194 210 6 177 224 7 169 219 8 174 234 9 193 209 10 197 215 MAX 198.0 234.0 MIN 166.0 201.0 AVG 183.3 216.0 In the table, the thrust detection method of SMT patch components is adopted, and two groups of 10 finished products are randomly selected for comparison, one group is the products before improvement, and the other group is the improved products obtained by adopting this application.
[0046] Observing the above content, among the improved products, product No. 1 with the smallest thrust value is better than product No. 4 with the largest thrust value before improvement.
[0047] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.
[0048] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An integrated inductor for enhancing electrode stability, comprising a hollow coil and a magnet, wherein both ends of the hollow coil are lead wires, characterized in that: The magnet is obtained by cold pressing magnetic powder, and the magnet includes a base and a columnar protrusion. One side of the base is symmetrically provided with an empty groove relative to the columnar protrusion, and the bottom surface of the base is provided with two grooves. The hollow coil is sleeved outside the columnar protrusion, and the lead wire is stripped of paint and flattened to obtain a connecting wire. The end of the connecting wire is connected to a flat electrode on the top surface of the base, and the flat electrode is bent twice and passed through the empty slot and then clamped in the groove to obtain an inductor intermediate; the inductor intermediate is placed in a mold, filled with magnetic powder material 2, and hot pressed to obtain an inductor; The particle size of the magnetic powder material 1 is 40-60 μm, the content of the epoxy insulating resin in the magnetic powder material 1 is 2.8-3.4% of the total weight of the magnetic powder material 1, the cold pressing temperature of the magnet is 35-45° C., and the pressure is 120-140 MPa; The particle size of the magnetic powder is 2-6 μm, the content of epoxy insulating resin in the magnetic powder is 0.8-1.2% of the total weight of the magnetic powder, the hot pressing temperature is 200-220° C., the pressure is 68-70 MPa, and the pressure holding time is 140-160 s.
2. The one-piece molded inductor with enhanced electrode stability as claimed in claim 1, characterized in that: The inner coil structure of the hollow coil matches the columnar protrusion, and the hollow coil is one layer or multiple layers.
3. The one-piece molded inductor with enhanced electrode stability as claimed in claim 2, characterized in that: A connecting groove is provided on the top surface of the base on the path where the pin line passes, and the connecting wire is pressed into the connecting groove and fixedly connected with the flat electrode.
4. The one-piece molded inductor with enhanced electrode stability as claimed in claim 3, characterized in that: The end of the connecting wire is bonded to the flat electrode by a filler-type conductive adhesive. The filler-type conductive adhesive comprises the following raw materials in parts by weight: 65-75 parts of epoxy resin, 4.6-5.6 parts of gold powder, 2-3 parts of graphite powder, 6-10 parts of solvent, and 1-2 parts of thixotropic agent.
5. The one-piece molded inductor with enhanced electrode stability as claimed in claim 2, characterized in that: The height of the columnar protrusion is 1-1.05 times the axial height of the hollow coil.
6. The one-piece molded inductor with enhanced electrode stability as claimed in claim 1, characterized in that: Magnetic powder 2: Preheat the hot pressing mold to 120-140°C before hot pressing.
7. The one-piece molded inductor with enhanced electrode stability as claimed in claim 6, characterized in that: The magnetic powder material 1 and the magnetic powder material 2 are both composed of metal powder, a binder and an additive, wherein the binder is epoxy resin, the metal powder is iron silicon chromium powder, and the additive is composed of SKF LGEM 2 and tungsten diselenide.
8. The one-piece molded inductor with enhanced electrode stability as claimed in claim 7, characterized in that: The content of the additive in the magnetic powder material 1 is 0.4-0.6% of the total weight of the magnetic powder material 1, and the weight ratio of SKF LGEM 2 and tungsten diselenide in the additive is 1:3-5; The content of the additive in the magnetic powder material 2 is 0.1-0.2% of the total weight of the magnetic powder material 1, and the weight ratio of SKF LGEM 2 and tungsten diselenide in the additive is 2:
1.
9. The one-piece molded inductor with enhanced electrode stability as claimed in claim 3, characterized in that: The thickness of the flat electrode is 1.2-1.4 times the depth of the connecting groove.
Citation Information
Patent Citations
Inductance element and manufacturing method
CN108389679A
Long-acting anti-oxidation high-conductivity conductive adhesive and preparation method thereof
CN112961626A
Integrally-formed inductor with high direct current superposition characteristic
CN113178312A
Integrated inductor
CN210039838U
Combined integrally-formed inductor
CN212062121U